Preparation method of novel high-strength and high-wear-resistance copper-tungsten composite material
The preparation of BNNS@Cu-W composite material through mechanical high-energy ball milling and molecular-level mixing technology was solved, and the problems of uneven dispersion of BNNS and insufficient thermal conductivity in copper tungsten alloy were achieved, and high strength, high wear resistance and good conductivity were achieved. Suitable for friction materials and abrasive electrode materials.
Patent Information
- Application Number
- CN202411089999.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art is difficult to achieve uniform dispersion and structural stability of BNNS in copper-tungsten alloys, resulting in insufficient wear resistance and electrical and thermal conductivity of copper-tungsten composite materials, especially in the application of friction materials and abrasive electrode materials.
The WO3@Cu composite powder was prepared by mechanical high-energy ball milling method, and the BNNS@CuO composite reinforcement was prepared by molecular-level mixing process, and then mixed with the WO3@Cu powder, and sintered and molded through a two-step reduction process to form BNNS@Cu-W Composite material ensures uniform dispersion and structural integrity of BNNS.
The high strength, high wear resistance and good thermal conductivity of copper tungsten alloy are achieved, and the dispersion problem of BNNS in copper tungsten matrix is solved, and the agglomeration and conductivity of tungsten particles are avoided, which provides high-performance copper tungsten alloy materials. Application guidance.
Smart Images

Figure CN118895437A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and specifically relates to a preparation method of a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy. Background Art
[0002] Copper-tungsten alloy is widely used in electronic packaging materials, abrasive electrode materials, brush materials and other fields because of its excellent mechanical properties and good electrical and thermal conductivity. With the rapid development of high-precision technologies such as new energy and microelectronics, higher requirements are placed on the wear resistance of copper-tungsten alloys used in brush materials and abrasive electrode materials. Since the discovery of two-dimensional boron nitride nanosheets (BNNS), compared with graphene, which is also a two-dimensional reinforcement, BNNS has excellent mechanical properties, high temperature resistance, high thermal conductivity, stronger chemical corrosion resistance, good self-lubrication and other excellent properties. Moreover, BNNS is not miscible with the copper-tungsten matrix, and while improving the wear resistance of copper-tungsten alloy, it will not reduce the high thermal conductivity and electrical conductivity of copper-tungsten alloy itself. Therefore, the use of BNNS as a reinforcement phase provides a new opportunity for the research and development of high-strength and high-wear-resistant copper-tungsten alloys.
[0003] At present, the preparation methods of BNNS reinforced metal matrix composites are relatively traditional, and it is impossible to prepare BNNS reinforced composites with excellent performance, uniform BNNS distribution and stable structure. Especially in the field of copper-tungsten alloy composites, so far, the research on adding BNNS to the copper-tungsten matrix to improve the friction performance of traditional copper-tungsten alloys is still in a blank field, and there is still a lack of effective methods to prepare copper-tungsten materials with uniform composition and limited tungsten particle growth. Therefore, the development of high-density and uniform copper-tungsten composite materials, while achieving good dispersion of BNNS in copper-tungsten alloys and structural integrity are still key scientific issues that need to be urgently solved for high-strength and high-wear-resistant copper-tungsten composite materials. Summary of the invention
[0004] Based on the above research background, the present invention proposes a method for preparing a new type of high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy. The method firstly adopts a mechanical high-energy ball milling method to prepare WO 3 @Cu composite powder, and then the BNNS@CuO composite reinforcement was prepared by molecular level mixing (MLM), and then the BNNS@CuO composite reinforcement was mixed with WO 3 @Cu powders are mixed and finally sintered to obtain BNNS@Cu-W composite materials. 3 The brittleness of WO can be further refined by high-energy ball milling. 3, improve the uneven dispersion of W particles in copper, and form a structure in which a soft phase (Cu) encapsulates a hard phase (W), and adopts a two-step reduction process to avoid the problem of tungsten particles growing in contact with each other during the subsequent reduction process; on the other hand, the preparation method effectively improves the dispersion of BNNS in the copper-tungsten matrix and retains the intrinsic structure of BNNS to the greatest extent. The preparation process is simple and low in cost, and can effectively solve the problems in the background technology. The copper-tungsten alloy prepared by this method not only has excellent wear resistance and mechanical properties, but also maintains good electrical and thermal conductivity, which provides technical guidance for the development of high-performance copper-tungsten alloy materials for abrasive electrode materials, brush materials, and friction materials.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] A novel method for preparing a high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy, the steps of which are as follows:
[0007] (1)WO 3 Preparation of @Cu composite powder
[0008] Weigh an appropriate amount of tungsten oxide powder (WO 3 ) and pure copper powder, WO 3 The powder was mixed with pure copper powder, and then the mixed powder and stainless steel balls were put into a stainless steel ball mill for high-energy ball milling to obtain WO 3 @Cu composite powder;
[0009] Further optimization, the specific operation of step (1) is:
[0010] Weigh 13g~25g of 50nm tungsten oxide powder (WO 3 ) and 80g~90g of dendrite pure copper powder, WO 3 The powder is ultrasonically dispersed in alcohol for 10 to 20 minutes, then mixed with pure copper powder, and the mixed solution is placed in a vacuum drying oven and heated to 70°C, and the mixed powder is obtained by vacuum drying. Subsequently, the mixed powder and stainless steel balls are placed in a stainless steel ball mill, argon (Ar) is used as a protective gas, 0.05wt% to 0.1wt% of stearic acid is added as a ball milling process control agent, and the ball-to-material ratio is 10:1 to 15:1; ball milling is performed for 6h to 12h to obtain WO 3 @Cu composite powder.
[0011] (2) Preparation of BNNS@CuO powder
[0012] Weigh 0.15g to 1.5g of boron nitride nanosheet (BNNS) powder and 7.5g to 75g of hydrated copper nitrate (Cu(NO 3 ) 2 ·3H2 O) were ultrasonically dispersed in deionized water for 10 min to 20 min. The solubility of hydrated copper nitrate in water is very high (125 g / 100 ml), which is convenient for the preparation of large quantities of powders. The BNNS dispersion solution was added to Cu(NO 3 ) 2 ·3H 2 O dispersed solution was stirred in a water bath at 50℃~80℃ for 30min to obtain BNNS / Cu(NO 3 ) 2 Mixed solution. Subsequently, 4.5g to 45g of sodium hydroxide (0.5mol / L) and 3.5g to 35g of glucose (0.8mol / L) were weighed and ultrasonically dispersed into an aqueous solution, and added to the above mixed solution and stirred. When the color of the solution changed from dark blue to brick red and a precipitate was formed, stirring was stopped, followed by suction filtration and vacuum drying at 70℃ to 80℃ to obtain BNNS@CuO powder.
[0013] (3) Preparation of BNNS@Cu-W composite powder
[0014] The powders obtained by (1) and (2) above were mixed and then placed in a stainless steel ball mill, Ar was introduced as a protective gas, 0.05wt% to 0.1wt% stearic acid was added as a ball milling process control agent, and the ball milling was performed for 4-8h to obtain a composite powder. The powder was then placed in a vacuum tube furnace and Ar / H was introduced. 2 The mixed gas is reduced in two steps to obtain BNNS@Cu-W composite powder. The reaction principle involved is shown in formula (1) and (2):
[0015] CuO+H 2 (g) →Cu+H 2 O(g) (1)
[0016] WO 3 + 3H 2 (g)→W + 3H 2 O(g) (2)
[0017] (4) Preparation of BNNS@Cu-W composite bulk
[0018] The BNNS@CuW composite powder was sintered in a fast hot pressing furnace (FHP) to obtain a BNNS@CuW composite block.
[0019] Further optimization, the specific operation of step (4) is:
[0020] The BNNS@Cu-W composite powder obtained in step (3) is filled in a mold, pre-pressed and then sintered in a fast hot pressing furnace (FHP) at a sintering temperature of 700 to 950°C and a heating rate of 50°C / min to 100°C / min. The sintering process is carried out under a vacuum state at a holding pressure of 100MPa to 200Mpa to obtain a BNNS@Cu-W composite block.
[0021] Preferably, in step (1), WO 3 Powder ratio: 16vt% to 32vt% (calculated by total amount); particle size 50nm; morphology can be spherical or quasi-spherical structure; the particle size of the pure copper powder is 20μm to 50μm; the shape is dendrite.
[0022] Preferably, in step (1), vacuum drying is performed using a vacuum drying oven with an operating temperature of ≤120°C.
[0023] Preferably, in step (1), the ball-to-material ratio is 15:1 to 20:1; and the ball milling speed is 500 r / min to 650 r / min.
[0024] Preferably, the proportion of BNNS powder in step (2) is: 0.15wt% to 1.5wt% (calculated by total amount); the sheet diameter is 100nm to 200nm; the morphology can be a single-layer, double-layer or multi-layer structure of boron nitride nanosheets.
[0025] Preferably, in step (2), Cu(NO 3 ) 2 ·3H 2 O was analytically pure (AR≥99%); NaOH was analytically pure (AR≥99%); glucose was analytically pure (AR≥99%).
[0026] Preferably, in step (3), the ball-to-material ratio is 5:1 to 10:1; and the ball milling speed is 150 r / min to 300 r / min.
[0027] Preferably, in step (3), the heating rate of the vacuum tube furnace is 5°C / min to 10°C / min, and the insulation temperatures of the two-step reduction are 300°C to 400°C and 600°C to 700°C respectively; the insulation time is 120min to 240min.
[0028] Beneficial effects of the present invention:
[0029] (1) The preparation method of boron nitride reinforced copper-tungsten alloy proposed in the present invention comprises the following steps: 3 The Cu-W matrix powder prepared by high energy mechanical ball milling can be refined by WO 3Achieve uniform distribution of W particles in the copper matrix and form a "soft (Cu) encapsulated hard (WO 3 )" structure to avoid WO 3 Aggregation and growth in the subsequent reduction process; on the other hand, the BNNS@Cu composite reinforcement prepared by the MLM method can reduce the density difference between the low-density BNNS and the copper-tungsten alloy matrix, and realize the uniform dispersion of BNNS in the copper-tungsten alloy matrix; and the solubility of BNNS in the copper-tungsten alloy matrix is extremely low, which will not affect the original electrical and thermal conductivity of the matrix;
[0030] (2) The two-step reduction process adopted by the method of the present invention for the composite powder can not only remove water vapor during the low-temperature reduction of CuO, but also prevent it from reacting with WO 3 The reaction produces tungsten fluoride (WO) which will coarsen W particles. 2 (OH) 2 ), and this process can also reduce the number of reduction times and avoid agglomeration caused by high-temperature phase migration to the greatest extent.
[0031] (3) The boron nitride reinforced copper-tungsten alloy prepared by the method of the present invention not only has a stable structure, a dense organization and a uniform composition, but also has excellent mechanical properties and wear resistance while still maintaining good electrical and thermal conductivity, thus achieving the successful development of a copper-tungsten alloy material with high comprehensive performance.
[0032] (4) The preparation method of the present invention has a short cycle and strong practicality, is convenient for mass production, and provides technical guidance for the development of high-performance copper-tungsten alloy materials for application in the field of power electronic materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced and explained below.
[0034] Figure 1 WO after ball milling in step (1) of Example 1 3 @Scanning electron microscope (SEM) image of Cu powder;
[0035] Figure 2 This is a scanning electron microscope image of the composite powder after reduction in step (3) of Example 1;
[0036] Figure 3 The conductivity and hardness bar graphs of BNNSs@Cu-W and BNNS / Cu-W materials in Example 1 and Comparative Example 1;
[0037] Figure 4 The stress-strain curves and friction coefficient change curves of BNNSs@Cu-W and BNNS / Cu-W materials in Example 1 and Comparative Example 1;
[0038] Figure 5 The conductivity and hardness bar graphs of BNNSs@Cu-W and BNNS / Cu-W materials in Example 2 and Comparative Example 2;
[0039] Figure 6 The stress-strain curves and friction coefficient change curves of BNNSs@Cu-W and BNNS / Cu-W materials in Example 2 and Comparative Example 2.
[0040] Figure 7 The conductivity and hardness bar graphs of BNNSs@Cu-W and BNNS / Cu-W materials in Example 3 and Comparative Example 3;
[0041] Figure 8 The stress-strain curves and friction coefficient change curves of BNNSs@Cu-W and BNNS / Cu-W materials in Example 3 and Comparative Example 3. DETAILED DESCRIPTION
[0042] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, wherein the methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified.
[0043] In the following embodiments:
[0044] The purity of BNNS powder is 99.9%, the number of layers is 5 to 20, the thickness is 5nm to 20nm, and the sheet diameter is 100nm to 200nm. Zhejiang Yamei Nanotechnology Co., Ltd.
[0045] Cu(NO 3 ) 2 ·3H 2 O, NaOH, and glucose were all analytical grade (AR ≥ 99%) and were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0046] The purity of Cu powder is 99.9%, the particle size is 20μm~50μm, and the morphology is dendritic. Shanghai Naio Nano Technology Co., Ltd.
[0047] Nano WO 3 The powder purity is 99.9%, the morphology is spherical, and the particle size is ~50nm, from Gerry Advanced Materials Co., Ltd.
[0048] Scanning electron microscope: Nova Nano-450, FEI, USA;
[0049] Mechanical properties of the BNNS@Cu-W and Cu-W alloy materials prepared in the examples and comparative examples were characterized by using a universal tensile testing machine (AUTOGRAPH AG-I, Shimadzu Corporation, Japan) to perform tensile tests at room temperature. The sample size (dog bone type) was 16 mm × 2 mm × 1.5 mm (length × width × thickness); the tensile rate was 0.18 mm / min.
[0050] Friction and wear properties of the BNNS@Cu-W and Cu-W alloy materials prepared in the examples and comparative examples were characterized as follows: Friction tests were conducted at room temperature using a friction and wear tester (MS-M9000, Lanzhou, China), where the test load was 10N to 15N and the rotation speed was 100r / min to 150r / min.
[0051] Example 1
[0052] A preparation method of a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy material, the specific steps are as follows:
[0053] (1)WO 3 Preparation of @Cu composite powder
[0054] Weigh 13g WO 3 powder and 90g of dendrite copper powder, WO 3 The powder was ultrasonically dispersed in alcohol for 20 minutes, then mixed with copper powder and dried in a vacuum drying oven at 70°C for 4 hours to obtain a mixed powder. The mixed powder and stainless steel balls were placed in a stainless steel ball mill with a ball-to-material ratio of 15:1, a rotation speed of 650r / min, Ar as a protective gas, and 0.1wt% stearic acid was added and ball milled for 12 hours to obtain WO 3 @Cu composite powder.
[0055] (2) Preparation of BNNS@CuO powder
[0056] Weigh 0.15 g of boron nitride nanosheets (BNNS) powder and 7.5 g of hydrated copper nitrate (Cu(NO 3 ) 2 ·3H 2 O) were ultrasonically dispersed in deionized water for 10 min, and the BNNS dispersion solution was added to Cu(NO 3 ) 2 ·3H 2 O dispersion solution and stirred in a 50 °C water bath for 30 min to obtain BNNS / Cu(NO 3 ) 2Mixed solution. Subsequently, 4.5 g of sodium hydroxide (0.5 mol / L) and 3.5 g of glucose (0.8 mol / L) were weighed and ultrasonically dispersed into an aqueous solution, and added to the above mixed solution and stirred. When the color of the solution changed from dark blue to brick red and a precipitate was generated, stirring was stopped, and then suction filtration and vacuum drying at 70°C were performed to obtain BNNS@CuO powder.
[0057] (3) Preparation of BNNS@Cu-W composite powder
[0058] The powders obtained by (1) and (2) above were mixed and then placed in a stainless steel ball mill, Ar was introduced as a protective gas, 0.05 wt% stearic acid was added as a ball milling process control agent, the rotation speed was 200 r / min, the ball-to-material ratio was 10:1, and the ball milling was performed for 4 h to obtain a composite powder. The powder was then placed in a vacuum tube furnace and Ar / H was introduced. 2 The mixed gas was reduced in two steps with a heating rate of 5°C / min. The first stage was kept at 300°C for 120 min, and the second stage was kept at 600°C for 120 min. BNNS@Cu-W composite powder was obtained.
[0059] (4) Preparation of BNNS@Cu-W composite bulk
[0060] The BNNS@Cu-W composite powder obtained in step (3) is filled in a mold, pre-pressed and then sintered in a fast hot pressing furnace (FHP) at a sintering temperature of 950°C, a pressure of 100 MPa, a heating rate of 100°C / min, and a heat preservation time of 10 min. The sintering process is carried out in a vacuum state to obtain a BNNS@Cu-W composite block.
[0061] By reducing the WO 3 The scanning characterization of BNNS@Cu composite powder and reduced BNNS@Cu-W powder revealed that after high-energy ball milling, WO 3 The particles are significantly finer than before ball milling, and WO 3 It is evenly "embedded" into the copper matrix to form a soft-hard structure. Moreover, after high-temperature reduction, the W particles did not agglomerate or grow. This indicates that during the reduction process, the copper wrapping prevented the W particles from growing in contact with each other.
[0062] Comparative Example 1
[0063] (1) Weigh 10 g of W powder with a particle size of 50 nm and 90 g of dendrite copper powder, ultrasonically disperse the W powder in alcohol for 20 min, then mix it with copper powder, and dry it in a vacuum drying oven at 70°C for 4 h to obtain a mixed powder. Put the mixed powder and stainless steel balls into a stainless steel ball mill with a ball-to-material ratio of 15:1, a rotation speed of 650 r / min, Ar as a protective gas, and add 0.1wt% stearic acid for ball milling for 12 h to obtain W@Cu composite powder.
[0064] (2) Weigh 0.15 g of boron nitride nanosheet (BNNS) powder and add it to the W@Cu composite powder obtained in the above step, then put it into a stainless steel ball mill, introduce Ar as a protective gas, add 0.1 wt% stearic acid as a ball milling process control agent, rotate at 200 r / min, and the ball-to-material ratio is 10:1. Ball milling is performed for 4 h to obtain BNNS@Cu-W composite powder.
[0065] (3) The BNNS@Cu-W composite powder obtained in step (2) is filled in a mold, pre-pressed, and then sintered in a fast hot pressing furnace (FHP) at a sintering temperature of 950°C, a pressure of 100 MPa, a heating rate of 100°C / min, and a heat preservation time of 10 min. The sintering process is carried out under a vacuum state to obtain a BNNS@Cu-W composite block.
[0066] If W particles are directly mixed with copper powder for high-energy ball milling, W particles will easily agglomerate, resulting in uneven dispersion, and will easily adhere and grow during the subsequent sintering process, reducing the strength of the material. 3 High-energy ball milling of powder and copper powder can 3 Break it up and form a "soft-encased hard" structure to achieve uniform dispersion and ensure that WO 3 The particles will not stick together and grow when wrapped in copper.
[0067] If BNNS is directly added to Cu-W powder and then low-energy ball milling is performed, this will result in uneven dispersion of BNNS in the Cu-W matrix, reducing the wettability between the two, resulting in reduced material strength and wear resistance. Therefore, the BNNS / CuO composite powder was prepared in advance by the MLM method, that is, BNNS was added to CuO in a uniformly dispersed state, and then ball milling was performed to achieve BNNS@CuO on WO 3 @The uniform dispersion of BNNS in the Cu-W matrix avoids the agglomeration problem caused by density difference, and achieves uniform dispersion of BNNS in the Cu-W matrix, as shown in step (1) in the embodiment.
[0068] The conductivity and hardness of the materials prepared in Example 1 and Comparative Example 1 were tested. The results are as follows: Figure 3As shown in the figure, compared with Example 1 and Comparative Example 1, the alloy material of Example 1 still maintains good electrical conductivity (about 87% IACS), which is 7% higher than that of the comparative example. As for hardness, Example 1 has a significant improvement over the material of Comparative Example 1, from 126HV to 183HV, an increase of about 45.2%. The main reason for this phenomenon is the dispersed distribution of W particles and the uniform dispersion of BNNS. The method of directly adding the reinforcing phase in the comparative example will cause the agglomeration of W particles and BNNS, increase the scattering effect on electrons and thus reduce the electrical conductivity.
[0069] The mechanical properties and friction and wear performance tests (10N, 100r / min) showed the following results: Figure 4 As shown. The tensile strength of the material in Example 1 is significantly improved compared with that of the material in Comparative Example 1, reaching 680MPa, and the elongation is also better than that of the material in Comparative Example 1. On the one hand, this is because the fine dispersed second phase W particles are evenly distributed, and have a strong Orowan strengthening effect, which improves the strength by hindering the movement of dislocations; on the other hand, compared with the agglomeration and growth of the reinforcing phase in Comparative Example 1, the uniformly dispersed reinforcement in the material in Example 1 also makes it have better plasticity, which is manifested as better elongation. For the friction coefficient, the material in Example 1 is reduced to 0.2 (the comparative example is 0.58), a decrease of about 65.5%. This is mainly attributed to the uniform distribution of BNNS, which allows the material to form a uniform self-lubricating film during the friction process, and the W particles dispersed on and around this self-lubricating film will help stabilize this film, thereby maximizing the wear resistance of BNNS.
[0070] Example 2
[0071] A preparation method of a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy material, the specific steps are as follows:
[0072] (1)WO 3 Preparation of @Cu composite powder
[0073] Weigh 13g WO 3 powder and 90g of dendrite copper powder, WO 3 The powder was ultrasonically dispersed in alcohol for 10 minutes, then mixed with pure copper powder and dried in a vacuum drying oven at 70°C for 4 hours to obtain a mixed powder. The mixed powder and stainless steel balls were placed in a stainless steel ball mill with a ball-to-material ratio of 20:1, a rotation speed of 500 r / min, Ar as a protective gas, and 0.05 wt% stearic acid was added and ball milled for 6 hours to obtain WO 3 @Cu composite powder.
[0074] (2) Preparation of BNNS@CuO powder
[0075] Weigh 1.5 g of boron nitride nanosheets (BNNS) powder and 75 g of hydrated copper nitrate (Cu(NO 3 ) 2 ·3H 2 O) were ultrasonically dispersed in deionized water for 20 min, and the BNNS dispersion solution was added to Cu(NO 3 ) 2 ·3H 2 O dispersion solution and stirred in a water bath at 80 °C for 30 min to obtain BNNS / Cu(NO 3 ) 2 Mixed solution. Subsequently, 45 g of sodium hydroxide (0.5 mol / L) and 35 g of glucose (0.8 mol / L) were weighed and ultrasonically dispersed into an aqueous solution, and added to the above mixed solution and stirred. When the color of the solution changed from dark blue to brick red and a precipitate was formed, stirring was stopped, and then suction filtration and vacuum drying at 80°C were performed to obtain BNNS@CuO powder.
[0076] (3) Preparation of BNNS@Cu-W composite powder
[0077] The powders obtained by (1) and (2) above were mixed and then placed in a stainless steel ball mill, Ar was introduced as a protective gas, 0.1 wt% stearic acid was added as a ball milling process control agent, the rotation speed was 300 r / min, the ball-to-material ratio was 5:1, and the ball milling was performed for 8 h to obtain a composite powder. The powder was then placed in a vacuum tube furnace and Ar / H was introduced. 2 The mixed gas was reduced in two steps with a heating rate of 10°C / min. The first stage was kept at 400°C for 240 min, and the second stage was kept at 700°C for 240 min. BNNS@Cu-W composite powder was obtained.
[0078] (4) Preparation of BNNS@Cu-W composite bulk
[0079] The BNNS@Cu-W composite powder obtained in step (3) is filled in a mold, pre-pressed and then sintered in a fast hot pressing furnace (FHP) at a sintering temperature of 700°C, a pressure of 200 MPa, a heating rate of 50°C / min, and a heat preservation time of 10 min. The sintering process is carried out under a vacuum state to obtain a BNNS@Cu-W composite block.
[0080] Comparative Example 2
[0081] (1) Weigh 10 g of W powder with a particle size of 50 nm and 90 g of dendrite copper powder, ultrasonically disperse the W powder in alcohol for 10 min, then mix it with copper powder, and dry it in a vacuum drying oven at 70°C for 4 h to obtain a mixed powder. Put the mixed powder and stainless steel balls into a stainless steel ball mill with a ball-to-material ratio of 20:1, a rotation speed of 500 r / min, Ar as a protective gas, and add 0.05wt% stearic acid for ball milling for 6 h to obtain W@Cu composite powder.
[0082] (2) Weigh 1.5 g of boron nitride nanosheet (BNNS) powder and add it to the W@Cu composite powder obtained in the above step, then put it into a stainless steel ball mill, introduce Ar as a protective gas, add 0.1 wt% stearic acid as a ball milling process control agent, rotate at 300 r / min, and the ball-to-material ratio is 5:1. Ball milling is performed for 8 h to obtain BNNS@Cu-W composite powder.
[0083] (3) The BNNS@Cu-W composite powder obtained in step (2) is filled in a mold, pre-pressed, and then sintered in a fast hot pressing furnace (FHP) at a sintering temperature of 700°C, a pressure of 200 MPa, a heating rate of 50°C / min, and a heat preservation time of 10 min. The sintering process is carried out in a vacuum state to obtain a BNNS@Cu-W composite block.
[0084] The conductivity and hardness of the materials prepared in Example 2 and Comparative Example 2 were tested. The results are as follows: Figure 3 As shown in the figure, compared with Example 1 and Comparative Example 1, the conductivity of both has a significant decrease (58.7% IACS; 49.2% IACS). The main reason is that the BNNS content is too high (1.5wt%), and it cannot be dispersed even by the MLM method. The serious agglomeration of BNNS leads to a significant enhancement of the scattering effect of the interface on electrons, resulting in a sharp decrease in conductivity.
[0085] The mechanical properties and friction and wear performance tests (10N, 100r / min) showed the following results: Figure 4 As shown. Compared with Example 1 and Comparative Example 1, the plasticity of the materials of Example 2 and Comparative Example 2 has decreased. The main reason is that the excessive content of BNNS leads to serious agglomeration, which causes debonding at the interface between BNNS and the matrix under stress, resulting in brittle fracture of the material; for the friction coefficient, the material of Example 2 is reduced to 0.25 (the comparative example is 0.53), which is not much different from the friction coefficient of the material of Example 1, but it can be clearly observed that the friction coefficient of the material of Example 2 fluctuates greatly. This is also due to the agglomeration of BNNS, which makes the generated self-lubricating film unstable, and the stress is easily concentrated at the interface during the friction process, causing BNNS to lose its original wear resistance.
[0086] Example 3
[0087] A preparation method of a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy material, the specific steps are as follows:
[0088] (1)WO 3 Preparation of @Cu composite powder
[0089] Weigh 25g WO 3 powder and 80g of dendrite copper powder, WO 3 The powder was ultrasonically dispersed in alcohol for 20 minutes, then mixed with copper powder and dried in a vacuum drying oven at 70°C for 4 hours to obtain a mixed powder. The mixed powder and stainless steel balls were placed in a stainless steel ball mill with a ball-to-material ratio of 17:1, a rotation speed of 600 r / min, Ar as a protective gas, and 0.1 wt% stearic acid was added and ball milled for 8 hours to obtain WO 3 @Cu composite powder.
[0090] (2) Preparation of BNNS@CuO powder
[0091] Weigh 1 g of boron nitride nanosheets (BNNS) powder and 40 g of hydrated copper nitrate (Cu(NO 3 ) 2 ·3H 2 O) were ultrasonically dispersed in deionized water for 15 min, and the BNNS dispersion solution was added to Cu(NO 3 ) 2 ·3H 2 O dispersion solution and stirred in a water bath at 80 °C for 30 min to obtain BNNS / Cu(NO 3 ) 2 Mixed solution. Subsequently, 20 g of sodium hydroxide (0.5 mol / L) and 2 g of glucose (0.8 mol / L) were weighed and ultrasonically dispersed into an aqueous solution, and added to the above mixed solution and stirred. When the color of the solution changed from dark blue to brick red and a precipitate was generated, stirring was stopped, and then suction filtration and vacuum drying at 75°C were performed to obtain BNNS@CuO powder.
[0092] (3) Preparation of BNNS@Cu-W composite powder
[0093] The powders obtained by (1) and (2) above were mixed and then placed in a stainless steel ball mill, Ar was introduced as a protective gas, 0.1 wt% stearic acid was added as a ball milling process control agent, the rotation speed was 150 r / min, the ball-to-material ratio was 7:1, and the ball milling was performed for 6 h to obtain a composite powder. The powder was then placed in a vacuum tube furnace and Ar / H was introduced. 2The mixed gas was reduced in two steps with a heating rate of 7°C / min. The first stage was kept at 350°C for 180 min, and the second stage was kept at 650°C for 180 min. BNNS@Cu-W composite powder was obtained.
[0094] (4) Preparation of BNNS@Cu-W composite bulk
[0095] The BNNS@Cu-W composite powder obtained in step (3) is filled in a mold, pre-pressed and sintered in a fast hot pressing furnace (FHP) at a sintering temperature of 800°C, a pressure of 150 MPa, a heating rate of 80°C / min, and a heat preservation time of 10 min. The sintering process is carried out in a vacuum state to obtain a BNNS@Cu-W composite block.
[0096] Comparative Example 3
[0097] (1) Weigh 20 g of W powder with a particle size of 50 nm and 80 g of dendrite copper powder, ultrasonically disperse the W powder in alcohol for 20 min, then mix it with copper powder, and dry it in a vacuum drying oven at 70°C for 4 h to obtain a mixed powder. Put the mixed powder and stainless steel balls into a stainless steel ball mill with a ball-to-material ratio of 17:1, a rotation speed of 600 r / min, Ar as a protective gas, and add 0.1wt% stearic acid for ball milling for 8 h to obtain W@Cu composite powder.
[0098] (2) Weigh 1 g of boron nitride nanosheet (BNNS) powder and add it to the W@Cu composite powder obtained in the above step, then put it into a stainless steel ball mill, introduce Ar as a protective gas, add 0.1 wt% stearic acid as a ball milling process control agent, rotate at 150 r / min, and the ball-to-material ratio is 7:1. Ball milling is performed for 6 h to obtain BNNS@Cu-W composite powder.
[0099] (3) The BNNS@Cu-W composite powder obtained in step (2) is filled in a mold, pre-pressed, and then sintered in a fast hot pressing furnace (FHP) at a sintering temperature of 800°C, a pressure of 150 MPa, a heating rate of 80°C / min, and a heat preservation time of 10 min. The sintering process is carried out in a vacuum state to obtain a BNNS@Cu-W composite block.
[0100] The conductivity and hardness of the composite materials prepared in Example 3 and Comparative Example 3 were tested. The results are as follows: Figure 7 As shown in the figure, because the W content of the material in Example 3 is doubled compared with that in Example 1, its conductivity is reduced (64.7% IACS). The main reason is that more reinforcements will produce more interfaces, which will enhance the scattering effect of electrons. The mechanical properties and friction and wear performance tests (15N, 150r / min) show the following results: Figure 8As shown, its enhancement mechanism is basically the same as that in Example 1.
[0101] In summary, the present invention provides a novel method for preparing high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy, and obtains a BNNS@Cu-W composite material with complete structure, dense organization and uniform dispersion. At room temperature, the friction coefficient of the BNNS@Cu-W composite material is only 0.2, the tensile strength is 683MPa, and the electrical conductivity is maintained above 87% IACS. The preparation method is simple, the experimental cycle is short and the practicability is strong. The obtained material has high strength and high wear resistance while still maintaining good electrical conductivity. Through the brittle phase WO 3 High-energy ball milling with Cu, adding BNNS using MLM technology, and generating W particles in situ during the reduction process to improve its dispersibility and interface bonding strength can effectively solve the problems in the background technology. The prepared copper-tungsten alloy material exhibits excellent mechanical properties and wear resistance, providing technical guidance for the development of high-performance copper-tungsten alloy materials for abrasive electrode materials, brush materials and friction materials.
[0102] The embodiments described above are only preferred embodiments of the present invention, rather than all embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art through any modification, replacement, improvement, etc. without any innovation are within the protection scope of the present invention.
Claims
1. A method for preparing a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy, characterized in that: The method steps are as follows: (1) Preparation of WO3@Cu composite powder Weigh appropriate amounts of tungsten oxide powder (WO3) and pure copper powder, mix the WO3 powder and pure copper powder by vacuum drying, and then put the mixed powder and stainless steel balls into a stainless steel ball mill for high-energy ball milling to obtain WO3@Cu composite powder; (2) Preparation of BNNS@CuO powder 0.15 g to 1.5 g of boron nitride nanosheet (BNNS) powder and 7.5 g to 75 g of hydrated copper nitrate (Cu(NO3)2·3H2O) were weighed and ultrasonically dispersed in deionized water, respectively, the dispersed solutions were mixed, and stirred in a water bath environment of 50°C to 80°C to obtain a BNNS / Cu(NO3)2 mixed solution; subsequently, 4.5 g to 45 g of sodium hydroxide (0.5 mol / L) and 3.5 g to 35 g of glucose (0.8 mol / L) were weighed and ultrasonically dispersed into aqueous solutions, and added to the above mixed solution and stirred, and stirring was stopped when a precipitate was generated, followed by suction filtration and vacuum drying to obtain BNNS@CuO powder; (3) Preparation of BNNS@Cu-W composite powder The powders obtained in (1) and (2) above were mixed, and then placed in a stainless steel ball mill, Ar was introduced as a protective gas, stearic acid was added as a ball milling process control agent, and the ball milling was performed for 4-8 hours to obtain a composite powder. The powder was then placed in a vacuum tube furnace, and Ar / H2 mixed gas was introduced for two-step reduction to obtain BNNS@Cu-W composite powder; (4) Preparation of BNNS@Cu-W composite bulk The BNNS@CuW composite powder was sintered into a BNNS@CuW composite block using a fast hot pressing furnace (FHP).
2. The method for preparing a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy according to claim 1, characterized in that: The specific operations of step (1) are: 13g-25g of tungsten oxide powder (WO3) with a particle size of 50nm and 80g-90g of dendrite pure copper powder are weighed, the WO3 powder is ultrasonically dispersed in alcohol for 10-20min, then mixed with pure copper powder, and a mixed powder is obtained by vacuum drying; then the mixed powder and stainless steel balls are loaded into a stainless steel ball mill, argon (Ar) is used as a protective gas, stearic acid is added as a ball milling process control agent, and high-energy ball milling is performed for 6h-12h to obtain WO3@Cu composite powder.
3. The method for preparing a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy according to claim 1 or 2, characterized in that: In step (1), the WO3 powder has a powder ratio of 16vt% to 32vt%, a particle size of 50nm, and a spherical or quasi-spherical shape; the pure copper powder has a particle size of 20μm to 50μm and a dendritic shape.
4. The method for preparing a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy according to claim 2, characterized in that: In step (1), the vacuum drying equipment is a vacuum drying oven, and its operating temperature is ≤120°C.
5. The method for preparing a novel high-strength and high-wear-resistant boron nitride reinforced tungsten alloy according to claim 1 or 2, characterized in that: In step (1), the ball-to-material ratio is 15:1 to 20:1; and the ball milling speed is 500 r / min to 650 r / min.
6. The method for preparing a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy according to claim 1 or 2, characterized in that: In step (2), the BNNS is a single-layer, double-layer or multi-layer boron nitride nanosheet; the Cu(NO3)2·3H2O, NaOH and glucose are all analytically pure (AR≥99%), and the vacuum drying temperature is 70-80°C.
7. The method for preparing a novel high-strength and high-wear-resistant boron nitride reinforced tungsten alloy according to claim 1 or 2, characterized in that: In step (3), the ball-to-material ratio is 5:1 to 10:1; and the ball milling speed is 150 r / min to 300 r / min.
8. The method for preparing a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy according to claim 1 or 2, characterized in that: In step (3), the vacuum reduction heating rate is 5°C / min to 10°C / min; the insulation temperatures of the two-step reduction are 300°C to 400°C and 600°C to 700°C respectively; and the insulation time is 120min to 240min.
9. The method for preparing a novel high-strength and high-wear-resistant boron nitride reinforced copper-tungsten alloy according to claim 1 or 2, characterized in that: The specific operation of step (4) is: The BNNS@Cu-W composite powder obtained in step (3) is filled in a mold, pre-pressed and then sintered in a fast hot pressing furnace (FHP) at a sintering temperature of 700 to 950°C and a heating rate of 50°C / min to 100°C / min. The sintering process is carried out under a vacuum state at a holding pressure of 100MPa to 200Mpa to obtain a BNNS@Cu-W composite block.
Citation Information
Cited By
Method for enhancing hardness of W-Cu composite material through W atomic cluster powder
CN122012980A