A composite reinforcing agent for asphalt pavement and preparation method thereof

By using a composite reinforcement of polyethylene, ethylene-vinyl acetate copolymer, polyethylene naphthalate, lignin fiber and gangue powder in asphalt pavement, combined with the synergistic effect of flocculent and granular lignin fibers, The problem of insufficient high temperature resistance and low temperature crack resistance of asphalt pavement is solved, and the high temperature resistance and crack resistance of asphalt pavement are significantly improved.

CN118702984BActive Publication Date: 2024-11-05TIANCHENG KENTELAI ZANHUANG TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411203339.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-05
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The existing asphalt pavement additives are not effective in improving the high temperature resistance and low temperature crack resistance of asphalt pavement, and cannot effectively prevent asphalt pavement from deforming in high temperature environments and cracking in low temperature environments.

Method used

Using a composite reinforcement, including polyethylene, ethylene-vinyl acetate copolymer, polyethylene naphthalate, lignin fiber, gangue powder and North American rock asphalt, through the synergy of flocculent and granular lignin fibers It can enhance the high-temperature resistance and low-temperature crack resistance of asphalt mixture, and improve dispersion and interaction by modifying gangue powder with carboxymethyl cellulose.

Benefits of technology

It significantly improves the high-temperature resistance and low-temperature crack resistance of asphalt pavement, extends the service life of the pavement, and enhances the stability of the asphalt mixture through the synergistic action of flocculent and granular lignin fibers and the modification of coal gangue powder. and bonding ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of additives for asphalt pavement, and proposes a composite reinforcing agent for asphalt pavement and a preparation method thereof. The composite reinforcing agent for asphalt pavement comprises the following components in parts by weight: 50 parts of polyethylene, 20-30 parts of ethylene-vinyl acetate copolymer, 15-35 parts of polyethylene naphthalate, 4-24 parts of lignin fiber, 15-25 parts of coal gangue powder, 6-12 parts of North American rock asphalt, and 2-6 parts of antioxidant. Through the above technical scheme, the problem of poor improvement of high temperature resistance and low temperature crack resistance of asphalt pavement by composite reinforcing agent for asphalt pavement in related technologies is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additives for asphalt pavement, and in particular to a composite reinforcing agent for asphalt pavement and a preparation method thereof. Background Art

[0002] Asphalt pavement refers to various types of pavement paved with asphalt materials mixed into mineral materials, which has many advantages. The asphalt pavement has a smooth surface and good driving comfort, and has good wear resistance and durability, and can withstand a large amount of traffic load and erosion from the natural environment. However, the long-term use of asphalt pavement will be repeatedly affected by vehicle loads, especially in low temperature environments, and the pavement is prone to cracks. In hot seasons, asphalt pavements are prone to high-temperature deformation. Therefore, improving the high temperature resistance and low-temperature cracking resistance of asphalt pavement is an urgent problem to be solved.

[0003] Usually, various additives are added to the asphalt mixture used in asphalt pavements to improve the performance of asphalt pavements. However, the performance of various asphalt pavement additives is relatively simple and the effect is not obvious. Although the commonly used asphalt pavement enhancers can improve the high temperature resistance of asphalt pavements to a certain extent, the effect is limited and cannot effectively prevent the asphalt pavement from deforming under high temperature conditions. In addition, when using conventional additives, the asphalt pavement has poor anti-cracking performance in low temperature environments. Therefore, the development of a composite enhancer for asphalt pavements to improve the high temperature resistance and low temperature anti-cracking performance of asphalt pavements is of great significance for extending the service life of the pavement. Summary of the invention

[0004] The present invention provides a composite reinforcing agent for asphalt pavement and a preparation method thereof, which solves the problem in the related art that the composite reinforcing agent for asphalt pavement has poor improvement on the high temperature resistance and low temperature cracking resistance of the asphalt pavement.

[0005] The technical solution of the present invention is as follows:

[0006] The present invention provides a composite reinforcing agent for asphalt pavement, comprising the following components in parts by weight:

[0007] 50 parts of polyethylene, 20-30 parts of ethylene-vinyl acetate copolymer, 15-35 parts of polyethylene naphthalate, 4-24 parts of lignin fiber, 15-25 parts of coal gangue powder, 6-12 parts of North American rock asphalt, and 2-6 parts of antioxidant.

[0008] As a further technical solution, the weight ratio of the polyethylene naphthalate to the lignin fiber is 2-3:1.

[0009] When the weight ratio of polyethylene naphthalate to lignin fiber is 2-3:1, the composite reinforcing agent for asphalt pavement can further improve the high temperature resistance and low temperature crack resistance of the asphalt pavement.

[0010] As a further technical solution, the lignin fibers are flocculent lignin fibers and granular lignin fibers.

[0011] When the lignin fiber is flocculent lignin fiber and granular lignin fiber, the flocculent lignin fiber has good dispersibility and filling property in asphalt mixture, can be effectively combined with asphalt in asphalt mixture, and can fill the tiny gaps in asphalt mixture, enhance the effective combination of asphalt and other mineral powders, and reduce the influence of temperature on the bonding ability of asphalt. While the granular lignin fiber promotes the effective combination of asphalt and other mineral powders, it can form a stable structural support in the asphalt mixture. Therefore, through the synergistic effect of flocculent lignin fiber and granular lignin fiber, the composite reinforcer for asphalt pavement can further improve the high temperature resistance and low temperature cracking resistance of asphalt pavement.

[0012] As a further technical solution, the weight ratio of the flocculent lignin fibers to the granular lignin fibers is 1-3:1.

[0013] When the weight ratio of the flocculent lignin fibers to the granular lignin fibers is 1 to 3:1, the composite reinforcing agent for asphalt pavement can further improve the high temperature resistance and low temperature crack resistance of the asphalt pavement.

[0014] As a further technical solution, the coal gangue powder is carboxymethyl cellulose modified coal gangue powder.

[0015] Surface modification of coal gangue powder using carboxymethyl cellulose can not only improve the dispersibility of coal gangue powder, but also strengthen the interaction with ethylene-vinyl acetate copolymer, polyethylene naphthalate and lignin fiber, thereby further improving the high temperature resistance and low temperature cracking resistance of asphalt pavement using composite reinforcing agent.

[0016] As a further technical solution, the preparation method of the carboxymethyl cellulose modified coal gangue powder includes the following steps: dissolving carboxymethyl cellulose in water to obtain a carboxymethyl cellulose solution, adding coal gangue powder to the carboxymethyl cellulose solution, dispersing evenly, and drying to obtain carboxymethyl cellulose modified coal gangue powder.

[0017] As a further technical solution, the weight ratio of the coal gangue powder to the carboxymethyl cellulose is 9-19:1.

[0018] When the weight ratio of coal gangue powder to carboxymethyl cellulose is 9-19:1, the composite reinforcing agent for asphalt pavement can further improve the high temperature resistance and low temperature crack resistance of the asphalt pavement.

[0019] As a further technical solution, the mass fraction of the carboxymethyl cellulose solution is 2% to 8%.

[0020] As a further technical solution, the antioxidant is one or both of antioxidant 1010 and antioxidant 168.

[0021] The present invention also provides a method for preparing the composite reinforcing agent for asphalt pavement, comprising the following steps: blending the components in parts by weight, extruding, and granulating to obtain the composite reinforcing agent for asphalt pavement.

[0022] As a further technical solution, during the extrusion, the temperature is 160-180°C.

[0023] The present invention also proposes the use of the composite reinforcing agent for asphalt pavement or the composite reinforcing agent for asphalt pavement prepared by the preparation method in asphalt pavement.

[0024] As a further technical solution, during the application, the weight ratio of the composite reinforcing agent for asphalt pavement to the asphalt mixture is 0.3~0.35:100.

[0025] The working principle and beneficial effects of the present invention are:

[0026] In the present invention, the composite reinforcing agent for asphalt pavement includes polyethylene naphthalate and lignin fiber. Polyethylene naphthalate has a semi-crystalline structure and has high temperature resistance. It can better react and fuse with asphalt mixture and absorb and disperse energy better when subjected to force. Lignin fiber can form a stable support structure and can effectively combine with polyethylene naphthalate. By using polyethylene naphthalate and lignin fiber together, the composite reinforcing agent for asphalt pavement can improve the high temperature resistance and low temperature crack resistance of asphalt pavement. In addition, the addition of coal gangue powder can also improve the high temperature resistance and low temperature crack resistance of asphalt pavement. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In the following embodiments and comparative examples, the model of polyethylene is LL6101XR; the model of ethylene-vinyl acetate copolymer is VS430; the model of polyethylene naphthalate is TN8065S; the particle size of coal gangue powder is 600 mesh; the length of flocculent lignin fiber is 2 mm, and the fiber spacing is 660 μm; the model of North American rock asphalt is 5U; the length of granular lignin fiber is 0.23 mm, and the particle size is 17 μm; the model of carboxymethyl cellulose is S14015.

[0029] Example 1

[0030] A composite reinforcing agent for asphalt pavement, comprising the following components in parts by weight:

[0031] 50 parts of polyethylene, 20 parts of ethylene-vinyl acetate copolymer, 15 parts of polyethylene naphthalate, 4 parts of lignin fiber, 15 parts of coal gangue powder, 6 parts of North American rock asphalt, and 2 parts of antioxidant 1010; wherein the lignin fiber is flocculent lignin fiber;

[0032] The preparation method thereof comprises the following steps:

[0033] The components in parts by weight are blended, extruded, and granulated to obtain a composite reinforcing agent for asphalt pavement;

[0034] During extrusion, the temperature of zone 1 is 160°C, the temperature of zone 2 is 180°C, and the temperature of zone 3 is 170°C.

[0035] Example 2

[0036] A composite reinforcing agent for asphalt pavement, comprising the following components in parts by weight:

[0037] 50 parts of polyethylene, 25 parts of ethylene-vinyl acetate copolymer, 23 parts of polyethylene naphthalate, 13 parts of lignin fiber, 20 parts of coal gangue powder, 9 parts of North American rock asphalt, and 4 parts of antioxidant 1010; wherein the lignin fiber is flocculent lignin fiber;

[0038] The preparation method thereof comprises the following steps:

[0039] The components in parts by weight are blended, extruded, and granulated to obtain a composite reinforcing agent for asphalt pavement;

[0040] During extrusion, the temperature of zone 1 is 160°C, the temperature of zone 2 is 180°C, and the temperature of zone 3 is 170°C.

[0041] Example 3

[0042] A composite reinforcing agent for asphalt pavement, comprising the following components in parts by weight:

[0043] 50 parts of polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 35 parts of polyethylene naphthalate, 24 parts of lignin fiber, 25 parts of coal gangue powder, 12 parts of North American rock asphalt, and 6 parts of antioxidant 1010; wherein the lignin fiber is flocculent lignin fiber;

[0044] The preparation method thereof comprises the following steps:

[0045] The components in parts by weight are blended, extruded, and granulated to obtain a composite reinforcing agent for asphalt pavement;

[0046] During extrusion, the temperature of zone 1 is 160°C, the temperature of zone 2 is 180°C, and the temperature of zone 3 is 170°C.

[0047] Example 4

[0048] The only difference between this embodiment and embodiment 2 is that 28 parts of polyethylene naphthalate and 8 parts of lignin fibers are added, wherein the lignin fibers are flocculent lignin fibers.

[0049] Example 5

[0050] The only difference between this embodiment and embodiment 2 is that 27 parts of polyethylene naphthalate and 9 parts of lignin fibers are added, wherein the lignin fibers are flocculent lignin fibers.

[0051] Example 6

[0052] The only difference between this embodiment and embodiment 2 is that 24 parts of polyethylene naphthalate and 12 parts of lignin fibers are added, wherein the lignin fibers are flocculent lignin fibers.

[0053] Example 7

[0054] The only difference between this embodiment and embodiment 6 is that the lignin fibers are granular lignin fibers.

[0055] Example 8

[0056] The only difference between this embodiment and embodiment 6 is that the lignin fibers are flocculent lignin fibers and granular lignin fibers, wherein the flocculent lignin fibers added are 4 parts and the granular lignin fibers added are 8 parts.

[0057] Example 9

[0058] The only difference between this embodiment and embodiment 6 is that the lignin fibers are flocculent lignin fibers and granular lignin fibers, wherein the flocculent lignin fibers added are 10 parts and the granular lignin fibers added are 2 parts.

[0059] Example 10

[0060] The only difference between this embodiment and embodiment 6 is that the lignin fibers are flocculent lignin fibers and granular lignin fibers, wherein 6 parts of flocculent lignin fibers are added and 6 parts of granular lignin fibers are added.

[0061] Embodiment 11

[0062] The only difference between this embodiment and embodiment 6 is that the lignin fibers are flocculent lignin fibers and granular lignin fibers, wherein 9 parts of flocculent lignin fibers are added and 3 parts of granular lignin fibers are added.

[0063] Example 12

[0064] The only difference between this embodiment and embodiment 11 is that the gangue powder is carboxymethyl cellulose modified gangue powder, and its preparation method comprises the following steps: dissolving 3 parts of carboxymethyl cellulose in water to obtain a carboxymethyl cellulose solution with a mass fraction of 5%, adding 17 parts of gangue powder to the 5% carboxymethyl cellulose solution with a mass fraction, stirring until the gangue powder is evenly dispersed, and concentrating to dryness to obtain carboxymethyl cellulose modified gangue powder.

[0065] Example 13

[0066] The only difference between this embodiment and embodiment 12 is that 19.5 parts of coal gangue powder and 0.5 parts of carboxymethyl cellulose are added, wherein the mass fraction of the carboxymethyl cellulose solution is 2%.

[0067] Embodiment 14

[0068] The only difference between this embodiment and embodiment 12 is that 18 parts of coal gangue powder and 2 parts of carboxymethyl cellulose are added.

[0069] Embodiment 15

[0070] The only difference between this embodiment and embodiment 12 is that 19 parts of coal gangue powder and 1 part of carboxymethyl cellulose are added.

[0071] Comparative Example 1

[0072] The only difference between this comparative example and Example 1 is that no lignin fiber is added and 19 parts of polyethylene naphthalate are added.

[0073] Comparative Example 2

[0074] The difference between this comparative example and Example 1 is that polyethylene naphthalate is not added and 19 parts of lignin fiber are added.

[0075] Comparative Example 3

[0076] The only difference between this comparative example and Example 1 is that no polyethylene naphthalate and no lignin fiber are added.

[0077] Comparative Example 4

[0078] The only difference between this comparative example and Example 1 is that no coal gangue powder is added.

[0079] The composite reinforcing agents for asphalt pavement of Examples 1 to 15 and Comparative Examples 1 to 4 were added to asphalt mixture (the weight ratio of the composite reinforcing agent for asphalt pavement to asphalt mixture was 0.35:100; wherein the content of 70# base asphalt in the asphalt mixture was 34wt%, and the content of limestone was 66wt%), and the following performance tests were performed according to the test method in JTG E20-2011 "Testing Procedures for Asphalt and Asphalt Mixtures for Highway Engineering":

[0080] High temperature rutting resistance test: Add the composite enhancer for asphalt pavement to the asphalt mixture, and test the rutting dynamic stability of the asphalt mixture; during the test, the temperature is 60°C and the wheel pressure is 0.7MPa;

[0081] Low temperature crack resistance test: Add the composite reinforcing agent for asphalt pavement to the asphalt mixture, and test the splitting tensile strength of the asphalt mixture; the temperature during the test is -10℃;

[0082] The test results are shown in Table 1 below:

[0083] Table 1 Test results

[0084]

[0085] Compared with Comparative Examples 1 to 3, the dynamic rutting stability and splitting tensile strength of the asphalt mixture of Example 1 are significantly improved, indicating that when the composite reinforcing agent for asphalt pavement includes polyethylene naphthalate and lignin fiber, polyethylene naphthalate and lignin fiber have a synergistic effect, which can make the composite reinforcing agent for asphalt pavement improve the high temperature resistance and low temperature cracking resistance of the asphalt pavement. Compared with Comparative Example 4, the dynamic rutting stability and splitting tensile strength of the asphalt mixture of Example 1 are significantly improved, indicating that the addition of coal gangue powder can also make the composite reinforcing agent for asphalt pavement improve the high temperature resistance and low temperature cracking resistance of the asphalt pavement.

[0086] Compared with Examples 2 and 4, the rutting dynamic stability and splitting tensile strength of the asphalt mixtures of Examples 5 to 6 are improved, indicating that when the weight ratio of polyethylene naphthalate to lignin fiber is 2 to 3:1, the composite reinforcing agent for asphalt pavement can further improve the high temperature resistance and low temperature cracking resistance of the asphalt pavement. Compared with Examples 6 to 7, the rutting dynamic stability and splitting tensile strength of the asphalt mixtures of Examples 8 to 11 are improved, indicating that when the lignin fiber is flocculent lignin fiber and granular lignin fiber, the composite reinforcing agent for asphalt pavement can further improve the high temperature resistance and low temperature cracking resistance of the asphalt pavement by using flocculent lignin fiber and granular lignin fiber together. Compared with Examples 8 to 9, the rutting dynamic stability and splitting tensile strength of the asphalt mixtures of Examples 10 to 11 are improved, indicating that when the weight ratio of flocculent lignin fiber to granular lignin fiber is 1 to 3:1, the composite reinforcing agent for asphalt pavement can further improve the high temperature resistance and low temperature cracking resistance of the asphalt pavement. Compared with Example 11, the rutting dynamic stability and splitting tensile strength of the asphalt mixtures of Examples 12 to 15 are improved, indicating that the surface modification of coal gangue powder by carboxymethyl cellulose can further improve the high temperature resistance and low temperature cracking resistance of the asphalt pavement by the composite reinforcing agent. In addition, compared with Examples 12 to 13, the rutting dynamic stability and splitting tensile strength of the asphalt mixtures of Examples 14 to 15 are improved, indicating that when the weight ratio of coal gangue powder to carboxymethyl cellulose is 9 to 19:1, the composite reinforcing agent for asphalt pavement can further improve the high temperature resistance and low temperature cracking resistance of the asphalt pavement.

[0087] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A composite reinforcing agent for asphalt pavement, characterized in that: The composition comprises the following components in parts by weight: 50 parts of polyethylene, 20-30 parts of ethylene-vinyl acetate copolymer, 15-35 parts of polyethylene naphthalate, 4-24 parts of lignin fiber, 15-25 parts of coal gangue powder, 6-12 parts of North American rock asphalt, and 2-6 parts of antioxidant; The lignin fibers are flocculent lignin fibers and granular lignin fibers.

2. A composite reinforcing agent for asphalt pavement according to claim 1, characterized in that: The weight ratio of the polyethylene naphthalate to the lignin fiber is 2-3:

1.

3. A composite reinforcing agent for asphalt pavement according to claim 1, characterized in that: The weight ratio of the flocculent lignin fibers to the granular lignin fibers is 1-3:

1.

4. The composite reinforcing agent for asphalt pavement according to claim 1, characterized in that: The coal gangue powder is carboxymethyl cellulose modified coal gangue powder.

5. A composite reinforcing agent for asphalt pavement according to claim 4, characterized in that: The preparation method of the carboxymethyl cellulose modified coal gangue powder comprises the following steps: dissolving carboxymethyl cellulose in water to obtain a carboxymethyl cellulose solution, adding coal gangue powder to the carboxymethyl cellulose solution, dispersing the mixture evenly, and drying the mixture to obtain the carboxymethyl cellulose modified coal gangue powder.

6. A composite reinforcing agent for asphalt pavement according to claim 5, characterized in that: The weight ratio of the coal gangue powder to the carboxymethyl cellulose is 9-19:

1.

7. A composite reinforcing agent for asphalt pavement according to claim 1, characterized in that: The antioxidant is one or both of antioxidant 1010 and antioxidant 168.

8. The method for preparing a composite reinforcing agent for asphalt pavement according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: blending the components in parts by weight, extruding, and granulating to obtain the composite reinforcing agent for asphalt pavement.

9. The method for preparing a composite reinforcing agent for asphalt pavement according to claim 8, characterized in that: During the extrusion, the temperature is 160-180°C.

Citation Information

Cited By

  • Green carbon-reducing modified asphalt, preparation method thereof and application of green carbon-reducing modified asphalt in high-doping-amount RAP

    CN119570274A