A kind of high temperature resistant zinc iron yellow pigment and preparation method thereof
Cobalt-doped zinc ferrate and N, C doped TiO2 composite materials were prepared by hydrothermal co-precipitation method, and composited with bismuth vanadate and coated with alumina on the surface, which solved the color change of existing high-temperature resistant zinc iron yellow pigments at high temperatures. Problem, bright colors and high catalytic activity are achieved, cost and toxicity are reduced, and are suitable for a variety of industrial applications.
Patent Information
- Application Number
- CN202411179953.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing high-temperature resistant zinc iron yellow pigments are prone to turn red or black under high temperature conditions, and the traditional methods are complex in technology, high in cost, and contain toxic substances, which cannot meet industrial needs.
Cobalt-doped zinc ferrate was prepared by hydrothermal co-precipitation method, and blended with N, C-doped TiO2, then uniformly recombined with bismuth vanadate, and the surface was coated with alumina, and high-temperature resistant zinc iron yellow was obtained by ball milling. pigment.
The pigment does not change color at 1500℃, has bright colors, and has high photocatalytic activity and catalytic activity. It solves the toxicity problem of traditional ceramic pigments, and is easy to separate and recover, with broad application prospects.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pigments, and in particular to a high temperature resistant zinc iron yellow pigment and a preparation method thereof. Background Art
[0002] Pigments are substances that color objects and are mainly used in industries such as coatings, inks, printing and dyeing, plastic products, rubber products, and ceramics. Pigments can generally be divided into organic pigments and inorganic pigments. It is well known that yellow iron oxide (chemical formula is Fe2O3·H2O) will dehydrate and transform into red iron (chemical formula is Fe2O3) when the temperature is higher than 170°C. However, there are many applications such as polyester paint, fluorocarbon coating, polyolefin plastic, rubber, silicone products, polyester film for window film, etc., whose ambient temperature is sometimes higher than 200°C, which can easily cause the fading of yellow iron oxide pigment.
[0003] Although ordinary high temperature resistant zinc iron yellow pigment can remain unchanged at 400℃, it has low tinting power, insufficient yellow phase, reddish, dark and dull color. U.S. Patent No. 2904395A introduces two methods for preparing zinc ferrite pigment: first, precipitate iron-containing and zinc-containing solutions by general methods, filter, wash, dry and calcine. Second, mix iron oxide hydrate and zinc oxide in a water suspension, calcine the mixture at a temperature of 750-1000℃ for 10-30min, and then slowly cool to 400-500℃ within 10min. In order to obtain bright color, it is necessary to react quickly during calcination to completely generate zinc ferrite, otherwise, sintering will occur. At the same time, in order to make the reaction proceed under appropriate conditions, a chlorine-containing catalyst, such as zinc chloride and hydrochloric acid, must be added. The disadvantage of this method is that the process line is long and the obtained pigment contains chloride, which is corrosive when used in coatings.
[0004] Chinese patent CN1554712A discloses a method for preparing zinc ferrite pigment, which comprises mixing iron powder with a particle size of less than 50 mesh and zinc powder according to weight percentage, ball milling activation, diluting with water, rusting and oxidizing to obtain zinc ferrite pigment powder. This method is relatively costly, and the rusting reaction in water is slow, the reaction cannot be guaranteed to proceed fully, and the zinc-iron content ratio cannot be guaranteed, thus affecting the color of the pigment.
[0005] Although the above-mentioned process methods have successfully prepared stable zinc ferrite pigment particles, their actual color is affected by the raw material ratio and preparation conditions. At the same time, they tend to turn red or black at 1000°C, so they cannot meet specific industrial needs. Summary of the invention
[0006] The purpose of the present invention is to provide a high temperature resistant zinc iron yellow pigment and a preparation method thereof, which does not change color even when heated to 1500°C and still maintains a bright yellow color. The pigment is not only brighter in color than traditional yellow ceramic pigments, but also solves the toxicity problem of traditional ceramic pigments. At the same time, the pigment has higher photocatalytic activity and catalytic activity, is ferromagnetic, is easy to separate and recycle, and has broad application prospects.
[0007] The technical solution of the present invention is achieved in this way:
[0008] The invention provides a method for preparing a high temperature resistant zinc iron yellow pigment. The method comprises the following steps: preparing cobalt-doped zinc ferrite by a hydrothermal coprecipitation method, mixing the cobalt-doped zinc ferrite with N and C-doped TiO2, then uniformly compounding the mixture with bismuth vanadate, coating the surface with aluminum oxide, and ball milling to obtain the high temperature resistant zinc iron yellow pigment.
[0009] As a further improvement of the present invention, the following steps are included:
[0010] S1. Preparation of cobalt-doped zinc ferrite: dissolving zinc salt, iron salt and cobalt salt in water, adding ammonia water to adjust the pH value of the solution, allowing the solution to stand for stratification, removing part of the supernatant, charging the viscous reactant into a reactor, reacting, cooling naturally after the reaction is completed, taking out the sample, filtering, washing and drying to obtain cobalt-doped zinc ferrite;
[0011] S2. Blending with N, C-doped TiO2: adding cobalt-doped zinc ferrite to water, adding urea and ammonia, stirring and mixing, dropping an ethanol solution of tetrabutyl titanate, stirring the reaction, filtering, washing, drying, and calcining to obtain a composite material of N, C-doped TiO2 and cobalt-doped zinc ferrite;
[0012] S3. Preparation of the composite: adding bismuth nitrate to concentrated nitric acid to obtain a solution A, dissolving ammonium metavanadate in an alkali solution, adding dropwise to the solution A, adjusting the pH value of the solution, adding the composite material obtained in step S2, heating and stirring the reaction, filtering, washing, and drying to obtain a composite;
[0013] S4. Coating: adding aluminum isopropoxide to ethyl acetate to obtain an oil phase; adding the complex and the emulsifier to water to obtain an aqueous phase; adding the aqueous phase dropwise to the oil phase, emulsifying, adjusting the pH value of the solution, stirring the reaction, filtering, washing, drying, and calcining to obtain a coated complex;
[0014] S5. Ball milling: ball mill the coated composite to obtain high temperature resistant zinc iron yellow pigment.
[0015] As a further improvement of the present invention, the molar ratio of the zinc salt, the iron salt and the cobalt salt in step S1 is 1:2:(0.01-0.02), the pH value of the adjustment solution is 9-11, the reaction temperature is 170-180°C, the reaction time is 5-7h, the zinc salt is at least one of zinc nitrate, zinc sulfate, and zinc chloride, the iron salt is at least one of ferric nitrate, ferric chloride, and ferric sulfate, and the cobalt salt is cobalt chloride.
[0016] As a further improvement of the present invention, the mass ratio of cobalt-doped zinc ferrite, urea, ammonia water, and tetrabutyl titanate in step S2 is 10: (0.5-1): (2-3): (3-5), the stirring reaction time is 2-4 hours, and the calcination temperature is 400-500° C. and the time is 2-4 hours.
[0017] As a further improvement of the present invention, the molar ratio of bismuth nitrate and ammonium metavanadate in step S3 is 1:1, the alkali solution is 2-3 mol / L NaOH or KOH solution, the concentration of concentrated nitric acid is 6-7 mol / L, the pH value of the adjusted solution is 6.2-6.5, the mass ratio of the composite material and bismuth nitrate is 10:3-4, the temperature of the heated and stirred reaction is 75-85°C, and the time is 0.5-1.5h.
[0018] As a further improvement of the present invention, the mass ratio of the aluminum isopropoxide, the complex and the emulsifier in step S4 is (4-6):10:(0.5-1), the emulsifier is selected from at least one of Tween-20, Tween-40, Tween-60, Tween-80 and Tween-85, the pH value of the adjusted solution is 9-10, the stirring reaction time is 2-3h, the calcination temperature is 500-600°C, and the time is 1-3h.
[0019] As a further improvement of the present invention, the ball milling time in step S5 is 2-4 hours.
[0020] The present invention further protects a high temperature resistant zinc iron yellow pigment prepared by the above preparation method.
[0021] The present invention has the following beneficial effects:
[0022] Zinc ferrite is a yellow pigment that can withstand a certain temperature, and has magnetic and photocatalytic properties. It can photocatalytically degrade organic matter or participate in organic catalytic reactions. At the same time, its pure yellow color also makes it a good pigment. However, it tends to turn red or black at 1000°C, which makes the pigment unable to withstand higher temperatures. The doped zinc ferrite prepared by cobalt doping in the present invention can improve the catalytic activity on the one hand, and on the other hand, cobalt replaces part of the iron, thereby improving the high temperature resistance of zinc ferrite.
[0023] Nitrogen and carbon doping can not only change the crystal structure of TiO2, but also inhibit the recombination rate of photogenerated electrons and holes. Compared with pure TiO2, the photocatalytic activity is significantly enhanced, so that TiO2 can use the visible light region for photocatalytic reaction and effectively decompose organic pollutants. At the same time, after mixing with N and C doped TiO2, the brightness of the yellow pigment is improved, making the yellow color brighter.
[0024] In addition, yellow ceramic pigments also include cadmium yellow (CdS), chrome yellow (PbCrO4, BaCrO4), antimony yellow (Sb2O5·2PbO), chrome titanium yellow [TiO2(Cr, Sb)], etc. However, they contain toxic heavy metal elements such as lead, chromium, and cadmium, and are highly toxic. Bismuth vanadate is a yellow pigment with excellent properties of being non-toxic, weather-resistant, bright in color, and environmentally friendly. However, pure bismuth vanadate yellow pigment becomes darker or even black when fired at above 600°C.
[0025] The present invention uniformly compounds a composite material of N, C doped TiO2 and cobalt doped zinc ferrite with bismuth vanadate, which not only reduces the cost of the pigment but also improves the catalytic activity. Alumina is further coated by a sol-gel method to generate alumina in situ, thereby improving the adhesion of the alumina on the pigment and thus improving the high temperature resistance of the pigment. Even if heated to 1500°C, the color will not change, thus overcoming the problem of high temperature discoloration of the yellow pigment and improving its stability.
[0026] The high temperature resistant zinc iron yellow pigment prepared by the invention does not change color even when heated to 1500°C and still maintains a bright yellow color. The pigment is not only brighter in color than traditional yellow ceramic pigments, but also solves the toxicity problem of traditional ceramic pigments. At the same time, it has higher photocatalytic activity and catalytic activity, is ferromagnetic, is easy to separate and recycle, and has broad application prospects. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] This embodiment provides a method for preparing a high temperature resistant zinc iron yellow pigment, which specifically comprises the following steps:
[0030] S1. Preparation of cobalt-doped zinc ferrite: 0.01 mol zinc chloride, 0.02 mol ferric chloride and 0.0001 mol cobalt chloride were dissolved in 200 mL water, and ammonia water was added dropwise to adjust the pH value of the solution to 9. The solution was allowed to stand for stratification, and part of the supernatant was removed. The viscous reactant was charged into a reactor, and stirred at 170° C. for 5 h. After the reaction was completed, the reaction was naturally cooled, the sample was taken out, filtered, washed, and dried to obtain cobalt-doped zinc ferrite;
[0031] S2. Blending with N, C-doped TiO2: Add 10 g of cobalt-doped zinc ferrite to 300 mL of water, add 0.5 g of urea and 2 g of ammonia water, stir and mix for 10 min, dropwise add 100 mL of ethanol solution containing 3 g of tetrabutyl titanate, stir and react for 2 h, filter, wash, dry, and calcine at 400 ° C for 2 h to obtain a composite material of N, C-doped TiO2 and cobalt-doped zinc ferrite;
[0032] S3. Preparation of the composite: 0.01 mol of bismuth nitrate was added to 100 mL of 6 mol / L concentrated nitric acid to obtain a solution A, 0.01 mol of ammonium metavanadate was dissolved in 100 mL of 2 mol / L NaOH solution, and the solution was added dropwise to solution A, the pH value of the solution was adjusted to 6.2, and the composite material prepared in step S2 was added, the mass ratio of the composite material to bismuth nitrate was 10:3, heated to 75 ° C, stirred for 0.5 h, filtered, washed, and dried to obtain a composite;
[0033] S4. Coating: 4 g of aluminum isopropoxide was added to 200 mL of ethyl acetate to obtain an oil phase; 10 g of the complex and 0.5 g of Tween-20 were added to 200 mL of water to obtain an aqueous phase; the aqueous phase was added dropwise to the oil phase, emulsified at 8000 r / min for 15 min, the pH value of the solution was adjusted to 9, the reaction was stirred for 2 h, filtered, washed, dried, and calcined at 500 ° C for 1 h to obtain a coated complex;
[0034] S5. Ball milling: ball mill the coated composite for 2 hours to obtain a high temperature resistant zinc iron yellow pigment.
[0035] Example 2
[0036] This embodiment provides a method for preparing a high temperature resistant zinc iron yellow pigment, which specifically comprises the following steps:
[0037] S1. Preparation of cobalt-doped zinc ferrite: 0.01 mol zinc sulfate, 0.02 mol iron sulfate and 0.0002 mol cobalt chloride were dissolved in 200 mL water, and ammonia water was added dropwise to adjust the pH value of the solution to 11. The solution was allowed to stand for stratification, and part of the supernatant was removed. The viscous reactant was charged into a reactor, and stirred at 180° C. for 7 h. After the reaction was completed, the reaction was naturally cooled, the sample was taken out, filtered, washed, and dried to obtain cobalt-doped zinc ferrite;
[0038] S2. Blending with N, C-doped TiO2: Add 10 g of cobalt-doped zinc ferrite to 300 mL of water, add 1 g of urea and 3 g of ammonia water, stir and mix for 10 min, dropwise add 100 mL of ethanol solution containing 5 g of tetrabutyl titanate, stir and react for 4 h, filter, wash, dry, and calcine at 500 ° C for 4 h to obtain a composite material of N, C-doped TiO2 and cobalt-doped zinc ferrite;
[0039] S3. Preparation of the composite: 0.01 mol of bismuth nitrate was added to 100 mL of 7 mol / L concentrated nitric acid to obtain a solution A, 0.01 mol of ammonium metavanadate was dissolved in 100 mL of 3 mol / L KOH solution, and the solution was added dropwise to solution A, the pH value of the solution was adjusted to 6.5, and the composite material prepared in step S2 was added, the mass ratio of the composite material to bismuth nitrate was 10:4, heated to 85 ° C, stirred for 1.5 h, filtered, washed, and dried to obtain a composite;
[0040] S4. Coating: 6 g of aluminum isopropoxide was added to 200 mL of ethyl acetate to obtain an oil phase; 10 g of the complex and 1 g of Tween-40 were added to 200 mL of water to obtain an aqueous phase; the aqueous phase was added dropwise to the oil phase, emulsified at 8000 r / min for 15 min, the pH value of the solution was adjusted to 10, the reaction was stirred for 3 h, filtered, washed, dried, and calcined at 600 ° C for 3 h to obtain a coated complex;
[0041] S5. Ball milling: ball mill the coated composite for 4 hours to obtain a high temperature resistant zinc iron yellow pigment.
[0042] Example 3
[0043] This embodiment provides a method for preparing a high temperature resistant zinc iron yellow pigment, which specifically comprises the following steps:
[0044] S1. Preparation of cobalt-doped zinc ferrite: 0.01 mol zinc nitrate, 0.02 mol iron nitrate and 0.00015 mol cobalt chloride were dissolved in 200 mL water, and ammonia water was added dropwise to adjust the pH value of the solution to 10. The solution was allowed to stand for stratification, and part of the supernatant was removed. The viscous reactant was charged into a reactor, and stirred at 175° C. for 6 h. After the reaction was completed, the reaction was naturally cooled, the sample was taken out, filtered, washed, and dried to obtain cobalt-doped zinc ferrite;
[0045] S2. Blending with N, C-doped TiO2: Add 10 g of cobalt-doped zinc ferrite to 300 mL of water, add 0.7 g of urea and 2.5 g of ammonia water, stir and mix for 10 min, dropwise add 100 mL of ethanol solution containing 4 g of tetrabutyl titanate, stir and react for 3 h, filter, wash, dry, and calcine at 450 ° C for 3 h to obtain a composite material of N, C-doped TiO2 and cobalt-doped zinc ferrite;
[0046] S3. Preparation of the composite: 0.01 mol of bismuth nitrate was added to 100 mL of 6.5 mol / L concentrated nitric acid to obtain a solution A, 0.01 mol of ammonium metavanadate was dissolved in 100 mL of 2.5 mol / L NaOH solution, and the solution was added dropwise to solution A, and the pH value of the solution was adjusted to 6.3, and the composite material prepared in step S2 was added, wherein the mass ratio of the composite material to bismuth nitrate was 10:3.5, and the reaction was heated to 80 ° C, stirred for 1 h, filtered, washed, and dried to obtain a composite;
[0047] S4. Coating: 5 g of aluminum isopropoxide was added to 200 mL of ethyl acetate to obtain an oil phase; 10 g of the complex and 0.7 g of Tween-80 were added to 200 mL of water to obtain an aqueous phase; the aqueous phase was added dropwise to the oil phase, emulsified at 8000 r / min for 15 min, the pH value of the solution was adjusted to 9.5, the reaction was stirred for 2.5 h, filtered, washed, dried, and calcined at 550° C. for 2 h to obtain a coated complex;
[0048] S5. Ball milling: ball mill the coated composite for 3 hours to obtain a high temperature resistant zinc iron yellow pigment.
[0049] Comparative Example 1
[0050] Compared with Example 3, the difference is that cobalt chloride is not added in step S1.
[0051] The details are as follows:
[0052] S1. Preparation of zinc ferrite: 0.01 mol zinc nitrate and 0.02 mol ferric nitrate were dissolved in 200 mL water, and ammonia water was added dropwise to adjust the pH value of the solution to 10. The solution was allowed to stand for stratification, and part of the supernatant was removed. The viscous reactant was charged into a reactor, and stirred at 175°C for 6 hours. After the reaction was completed, the reaction was naturally cooled, and the sample was taken out, filtered, washed, and dried to obtain zinc ferrite.
[0053] S2. Blending with N, C-doped TiO2: 10 g of zinc ferrite was added to 300 mL of water, 0.7 g of urea and 2.5 g of ammonia water were added, and the mixture was stirred for 10 min. 100 mL of an ethanol solution containing 4 g of tetrabutyl titanate was added dropwise, and the mixture was stirred for 3 h. The mixture was filtered, washed, dried, and calcined at 450 ° C for 3 h to obtain a composite material of N, C-doped TiO2 and zinc ferrite.
[0054] S3. Preparation of the composite: 0.01 mol of bismuth nitrate was added to 100 mL of 6.5 mol / L concentrated nitric acid to obtain a solution A, 0.01 mol of ammonium metavanadate was dissolved in 100 mL of 2.5 mol / L NaOH solution, and the solution was added dropwise to solution A, and the pH value of the solution was adjusted to 6.3, and the composite material prepared in step S2 was added, wherein the mass ratio of the composite material to bismuth nitrate was 10:3.5, and the reaction was heated to 80 ° C, stirred for 1 h, filtered, washed, and dried to obtain a composite;
[0055] S4. Coating: 5 g of aluminum isopropoxide was added to 200 mL of ethyl acetate to obtain an oil phase; 10 g of the complex and 0.7 g of Tween-80 were added to 200 mL of water to obtain an aqueous phase; the aqueous phase was added dropwise to the oil phase, emulsified at 8000 r / min for 15 min, the pH value of the solution was adjusted to 9.5, the reaction was stirred for 2.5 h, filtered, washed, dried, and calcined at 550° C. for 2 h to obtain a coated complex;
[0056] S5. Ball milling: ball mill the coated composite for 3 hours to obtain a high temperature resistant zinc iron yellow pigment.
[0057] Comparative Example 2
[0058] Compared with Example 3, the difference is that urea is not added in step S2.
[0059] The details are as follows:
[0060] S1. Preparation of cobalt-doped zinc ferrite: 0.01 mol zinc nitrate, 0.02 mol iron nitrate and 0.00015 mol cobalt chloride were dissolved in 200 mL water, and ammonia water was added dropwise to adjust the pH value of the solution to 10. The solution was allowed to stand for stratification, and part of the supernatant was removed. The viscous reactant was charged into a reactor, and stirred at 175° C. for 6 h. After the reaction was completed, the reaction was naturally cooled, the sample was taken out, filtered, washed, and dried to obtain cobalt-doped zinc ferrite;
[0061] S2. Blending with TiO2: 10 g of cobalt-doped zinc ferrite was added to 300 mL of water, 2.5 g of ammonia water was added, the mixture was stirred for 10 min, 100 mL of an ethanol solution containing 4 g of tetrabutyl titanate was added dropwise, the mixture was stirred for 3 h, filtered, washed, dried, and calcined at 450 ° C for 3 h to obtain a composite material of TiO2 and cobalt-doped zinc ferrite;
[0062] S3. Preparation of the composite: 0.01 mol of bismuth nitrate was added to 100 mL of 6.5 mol / L concentrated nitric acid to obtain a solution A, 0.01 mol of ammonium metavanadate was dissolved in 100 mL of 2.5 mol / L NaOH solution, and the solution was added dropwise to solution A, and the pH value of the solution was adjusted to 6.3, and the composite material prepared in step S2 was added, wherein the mass ratio of the composite material to bismuth nitrate was 10:3.5, and the reaction was heated to 80 ° C, stirred for 1 h, filtered, washed, and dried to obtain a composite;
[0063] S4. Coating: 5 g of aluminum isopropoxide was added to 200 mL of ethyl acetate to obtain an oil phase; 10 g of the complex and 0.7 g of Tween-80 were added to 200 mL of water to obtain an aqueous phase; the aqueous phase was added dropwise to the oil phase, emulsified at 8000 r / min for 15 min, the pH value of the solution was adjusted to 9.5, the reaction was stirred for 2.5 h, filtered, washed, dried, and calcined at 550° C. for 2 h to obtain a coated complex;
[0064] S5. Ball milling: ball mill the coated composite for 3 hours to obtain a high temperature resistant zinc iron yellow pigment.
[0065] Comparative Example 3
[0066] Compared with Example 3, the difference is that step S2 is not performed.
[0067] The details are as follows:
[0068] S1. Preparation of cobalt-doped zinc ferrite: 0.01 mol zinc nitrate, 0.02 mol iron nitrate and 0.00015 mol cobalt chloride were dissolved in 200 mL water, and ammonia water was added dropwise to adjust the pH value of the solution to 10. The solution was allowed to stand for stratification, and part of the supernatant was removed. The viscous reactant was charged into a reactor, and stirred at 175° C. for 6 h. After the reaction was completed, the reaction was naturally cooled, the sample was taken out, filtered, washed, and dried to obtain cobalt-doped zinc ferrite;
[0069] S2. Preparation of the complex: 0.01 mol of bismuth nitrate was added to 100 mL of 6.5 mol / L concentrated nitric acid to obtain solution A, 0.01 mol of ammonium metavanadate was dissolved in 100 mL of 2.5 mol / L NaOH solution, and the solution was added dropwise to solution A, the pH value of the solution was adjusted to 6.3, cobalt-doped zinc ferrite was added, the mass ratio of the cobalt-doped zinc ferrite to bismuth nitrate was 10:3.5, heated to 80 ° C, stirred for 1 h, filtered, washed, and dried to obtain a complex;
[0070] S3. Coating: 5 g of aluminum isopropoxide was added to 200 mL of ethyl acetate to obtain an oil phase; 10 g of the complex and 0.7 g of Tween-80 were added to 200 mL of water to obtain an aqueous phase; the aqueous phase was added dropwise to the oil phase, emulsified at 8000 r / min for 15 min, the pH value of the solution was adjusted to 9.5, the reaction was stirred for 2.5 h, filtered, washed, dried, and calcined at 550° C. for 2 h to obtain a coated complex;
[0071] S4. Ball milling: ball mill the coated composite for 3 hours to obtain a high temperature resistant zinc iron yellow pigment.
[0072] Comparative Example 4
[0073] Compared with Example 3, the difference is that step S3 is not performed.
[0074] The details are as follows:
[0075] S1. Preparation of cobalt-doped zinc ferrite: 0.01 mol zinc nitrate, 0.02 mol iron nitrate and 0.00015 mol cobalt chloride were dissolved in 200 mL water, and ammonia water was added dropwise to adjust the pH value of the solution to 10. The solution was allowed to stand for stratification, and part of the supernatant was removed. The viscous reactant was charged into a reactor, and stirred at 175° C. for 6 h. After the reaction was completed, the reaction was naturally cooled, the sample was taken out, filtered, washed, and dried to obtain cobalt-doped zinc ferrite;
[0076] S2. Blending with N, C-doped TiO2: Add 10 g of cobalt-doped zinc ferrite to 300 mL of water, add 0.7 g of urea and 2.5 g of ammonia water, stir and mix for 10 min, dropwise add 100 mL of ethanol solution containing 4 g of tetrabutyl titanate, stir and react for 3 h, filter, wash, dry, and calcine at 450 ° C for 3 h to obtain a composite material of N, C-doped TiO2 and cobalt-doped zinc ferrite;
[0077] S3. Coating: 5 g of aluminum isopropoxide was added to 200 mL of ethyl acetate to obtain an oil phase; 10 g of the composite material obtained in step S2 and 0.7 g of Tween-80 were added to 200 mL of water to obtain an aqueous phase; the aqueous phase was added dropwise to the oil phase, emulsified at 8000 r / min for 15 min, the pH value of the solution was adjusted to 9.5, the reaction was stirred for 2.5 h, filtered, washed, dried, and calcined at 550 ° C for 2 h to obtain a coated composite material;
[0078] S4. Ball milling: ball mill the coated composite material for 3 hours to obtain a high temperature resistant zinc iron yellow pigment.
[0079] Comparative Example 5
[0080] Compared with Example 3, the difference is that step S4 is not performed.
[0081] The details are as follows:
[0082] S1. Preparation of cobalt-doped zinc ferrite: 0.01 mol zinc nitrate, 0.02 mol iron nitrate and 0.00015 mol cobalt chloride were dissolved in 200 mL water, and ammonia water was added dropwise to adjust the pH value of the solution to 10. The solution was allowed to stand for stratification, and part of the supernatant was removed. The viscous reactant was charged into a reactor, and stirred at 175° C. for 6 h. After the reaction was completed, the reaction was naturally cooled, the sample was taken out, filtered, washed, and dried to obtain cobalt-doped zinc ferrite;
[0083] S2. Blending with N, C-doped TiO2: Add 10 g of cobalt-doped zinc ferrite to 300 mL of water, add 0.7 g of urea and 2.5 g of ammonia water, stir and mix for 10 min, dropwise add 100 mL of ethanol solution containing 4 g of tetrabutyl titanate, stir and react for 3 h, filter, wash, dry, and calcine at 450 ° C for 3 h to obtain a composite material of N, C-doped TiO2 and cobalt-doped zinc ferrite;
[0084] S3. Preparation of the composite: 0.01 mol of bismuth nitrate was added to 100 mL of 6.5 mol / L concentrated nitric acid to obtain a solution A, 0.01 mol of ammonium metavanadate was dissolved in 100 mL of 2.5 mol / L NaOH solution, and the solution was added dropwise to solution A, and the pH value of the solution was adjusted to 6.3, and the composite material prepared in step S2 was added, wherein the mass ratio of the composite material to bismuth nitrate was 10:3.5, and the reaction was heated to 80 ° C, stirred for 1 h, filtered, washed, and dried to obtain a composite;
[0085] S4. Ball milling: ball mill the composite for 3 hours to obtain a high temperature resistant zinc iron yellow pigment.
[0086] Test Example 1 Temperature resistance test
[0087] The high temperature resistant zinc iron yellow pigment samples prepared in Examples 1-3 and Comparative Examples 1-5 were tested for the heat resistance of the pigment powder according to the national standard HG / T 3853-2006 Pigment Dry Powder Heat Resistance Determination Method, and the test temperature was set to 1000 and 1500°C. Specific operation: the oven temperature was raised to the set temperature, and after the oven temperature was stable, a crucible containing 2.5g of the sample powder to be tested was placed in the oven, and the timing was started when the oven temperature was raised to the set temperature, and the sample was taken out after 30 minutes, and the color difference ΔE of the pigment before and after baking was measured after the sample was cooled.
[0088] The results are shown in Table 1.
[0089] Table 1:
[0090]
[0091] It can be seen from the above table that the high temperature resistant zinc iron yellow pigments prepared in Examples 1-3 of the present invention have good high temperature resistance.
[0092] Test Example 2
[0093] In the light / ultrasound-Fenton system degradation antibiotic experiment, the illumination condition uses an iodine tungsten lamp with a power of 200W as the light source, and the ultrasonic power is 100W under the ultrasonic condition. Weigh 10mg of the high temperature resistant zinc iron yellow pigment obtained in Examples 1-3 and Comparative Examples 1-5 in 50mL 20mg / L tetracycline hydrochloride solution, react for 60min in a light-proof environment, and then react for 80min under light ultrasonication. The distance between the iodine tungsten lamp and the tetracycline hydrochloride solution is about 30cm and remains unchanged. After the reaction is completed, centrifuge separation is performed using a centrifuge, and the catalyst absorbance is read at a wavelength of 357nm using an ultraviolet spectrophotometer to calculate the degradation rate of the target pollutant: k=(1-C / C0)×100%. In the calculation formula, C0 represents the initial concentration of the antibiotic, and C represents the concentration of the antibiotic at different times. When other conditions are the same, the concentration can be replaced by the value of the absorbance to calculate the degradation rate, that is, C / C0=A / A0.
[0094] The results are shown in Table 2.
[0095] Table 2:
[0096]
[0097] It can be seen from the above table that the high temperature resistant zinc iron yellow pigments prepared in Examples 1-3 of the present invention have good photocatalytic degradation performance.
[0098] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a high temperature resistant zinc iron yellow pigment, It is characterized in that Cobalt-doped zinc ferrite was prepared by hydrothermal coprecipitation. Cobalt-doped zinc ferrite and N, C-doped TiO 2 The mixture is mixed, then uniformly compounded with bismuth vanadate, the surface is coated with aluminum oxide, and ball milled to obtain a high temperature resistant zinc iron yellow pigment, which specifically includes the following steps: S1. Preparation of cobalt-doped zinc ferrite: dissolving zinc salt, iron salt and cobalt salt in water, adding ammonia water to adjust the pH value of the solution, allowing the solution to stand for stratification, removing part of the supernatant, charging the viscous reactant into a reactor, reacting, cooling naturally after the reaction is completed, taking out the sample, filtering, washing and drying to obtain cobalt-doped zinc ferrite; S2. TiO doped with N and C 2 Mixing: Add cobalt-doped zinc ferrite into water, add urea and ammonia water, stir and mix evenly, drop ethanol solution of tetrabutyl titanate, stir and react, filter, wash, dry, and calcine to obtain N, C-doped TiO 2 Composite materials with cobalt-doped zinc ferrite; S3. Preparation of the composite: adding bismuth nitrate to concentrated nitric acid to obtain a solution A, dissolving ammonium metavanadate in an alkali solution, adding dropwise to the solution A, adjusting the pH value of the solution, adding the composite material obtained in step S2, heating and stirring the reaction, filtering, washing, and drying to obtain a composite; S4. Coating: adding aluminum isopropoxide to ethyl acetate to obtain an oil phase; adding the complex and the emulsifier to water to obtain an aqueous phase; adding the aqueous phase dropwise to the oil phase, emulsifying, adjusting the pH value of the solution, stirring the reaction, filtering, washing, drying, and calcining to obtain a coated complex; S5. Ball milling: ball mill the coated composite to obtain high temperature resistant zinc iron yellow pigment.
2. The preparation method according to claim 1, It is characterized in that The molar ratio of the zinc salt, the iron salt and the cobalt salt in step S1 is 1:2:(0.01-0.02), the pH value of the adjustment solution is 9-11, the reaction temperature is 170-180°C, the reaction time is 5-7h, the zinc salt is at least one of zinc nitrate, zinc sulfate, and zinc chloride, the iron salt is at least one of iron nitrate, iron chloride, and iron sulfate, and the cobalt salt is cobalt chloride.
3. The preparation method according to claim 1, It is characterized in that In step S2, the mass ratio of cobalt-doped zinc ferrite, urea, ammonia water, and tetrabutyl titanate is 10:(0.5-1):(2-3):(3-5), the stirring reaction time is 2-4 hours, and the calcination temperature is 400-500° C. and the time is 2-4 hours.
4. The preparation method according to claim 1, It is characterized in that In step S3, the molar ratio of bismuth nitrate to ammonium metavanadate is 1:1, the alkali solution is a 2-3 mol / L NaOH or KOH solution, the concentration of concentrated nitric acid is 6-7 mol / L, the pH value of the adjusted solution is 6.2-6.5, the mass ratio of the composite material to bismuth nitrate is 10:3-4, the temperature of the heated and stirred reaction is 75-85°C, and the time is 0.5-1.5h.
5. The preparation method according to claim 1, It is characterized in that The mass ratio of the aluminum isopropoxide, the complex and the emulsifier in step S4 is (4-6):10:(0.5-1), the emulsifier is selected from at least one of Tween-20, Tween-40, Tween-60, Tween-80 and Tween-85, the pH value of the adjusted solution is 9-10, the stirring reaction time is 2-3h, the calcination temperature is 500-600°C, and the time is 1-3h.
6. The preparation method according to claim 1, It is characterized in that The ball milling time in step S5 is 2-4 hours.
7. A high temperature resistant zinc iron yellow pigment obtained by the preparation method according to any one of claims 1 to 6.