Preparation of graphene oxide in-situ modified inorganic phosphate binder and application of graphene oxide in-situ modified inorganic phosphate binder in bonding solid lubricating coating in wide temperature range

Through the chemical reaction of graphene oxide and phosphate binder, a dense and flexible composite coating is formed, which solves the problem of insufficient friction coefficient and wear resistance of existing high-temperature lubricating materials in a wide temperature range, and realizes Highly efficient lubrication performance.

CN118703115APending Publication Date: 2024-09-27LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES

Patent Information

Application Number
CN202410722236.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

It is difficult for existing high-temperature lubricating materials to maintain a stable friction coefficient and excellent wear resistance in a wide temperature range, and the lubricating materials are very sensitive to temperature and cannot achieve continuous, reliable and multi-cycle lubrication in a wide temperature range.

Method used

Through the chemical reaction between the oxygen-containing groups on the surface of graphene oxide and the phosphate ions in the phosphate binder, graphene oxide is introduced into the phosphate molecular network structure in situ to form a denser and more flexible composite coating, which is combined with The lubricating fillers are mixed to prepare a wide temperature range bonded solid lubricating coating.

Benefits of technology

It significantly improves the density and flexibility of the coating, reduces the friction coefficient, and especially has excellent friction coefficient at high temperatures, prolongs the wear life, and simplifies the preparation process to facilitate industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118703115A
    Figure CN118703115A
Patent Text Reader

Abstract

The invention discloses preparation of a graphene oxide in-situ modified inorganic phosphate binder and application of the graphene oxide in-situ modified inorganic phosphate binder in bonding a solid lubricating coating in a wide temperature range. According to the preparation method, lamellar graphene oxide is introduced into a molecular network structure of an inorganic phosphate binder in situ from a molecular level by mainly utilizing reactivity of oxygen-containing groups on the edge and the surface of graphene oxide and the inorganic phosphate binder, so that the flexibility of the inorganic phosphate binder is remarkably improved; and meanwhile, the crosslinking density of the inorganic phosphate binder is improved, the compactness is improved, and the average friction coefficient and the wear rate of the composite coating in the wide temperature range of 25-600 DEG C are remarkably reduced. The graphene oxide in-situ modified inorganic phosphate binder prepared by the method disclosed by the invention has huge application potential in the field of wide-temperature-range solid lubricating coating bonding, and can be used for solving the technical problems of long-term surface lubricating protection, burning sticking prevention and the like of related mechanical equipment under a wide-temperature-range service working condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation of an in-situ modified inorganic phosphate binder of graphene oxide and its application in a wide temperature range bonded solid lubricating coating, belonging to the technical field of bonded solid lubrication. Background Art

[0002] High-temperature lubrication is widely used in modern industrial fields such as aerospace, nuclear energy, metallurgy and metal processing. It is usually also the key bottleneck restricting the reliability, service life and operating efficiency of high-temperature motion systems in these fields. Especially in recent years, with the rapid development of industrial technology, the service temperature of related mechanical equipment has become higher and higher, and the service temperature range it faces is also getting wider and wider. On the one hand, this requires that the use temperature of lubricating materials must also be higher and higher. At the same time, it requires that lubricating materials also have good lubrication properties in medium and low temperature environments, and can achieve continuous, reliable and multi-cycle lubrication in a wide temperature range from room temperature to 800°C, that is, wide temperature range self-lubrication. The main challenge faced by wide temperature range lubricating coating materials is that lubricating materials are very sensitive to temperature. Each lubricating material has its specific operating temperature range. So far, no single solid lubricating material has been found that has a stable friction coefficient and excellent wear resistance in a wide temperature range.

[0003] The Chinese invention patent (CN202310625922.0) discloses a carbon fiber grafted graphene oxide modified phosphate bonding coating and its preparation method and application, which mainly grafts graphene oxide to the surface of carbon fiber to form a dendritic structure, making its surface rougher, thereby enhancing the interface bonding between the carbon fiber-graphene oxide reinforcement phase and other components in the phosphate bonding coating, and ultimately improving the wear resistance of the coating. The core technology of the above patent is to improve the dispersibility of the carbon fiber reinforcement phase in the phosphate binder by modifying the carbon fiber with graphene oxide, but the two are simply physically blended, there is no chemical bond, and there is still a problem of phase interface difference. Summary of the invention

[0004] The present invention aims to provide a method for preparing an inorganic phosphate binder modified in situ by graphene oxide, and utilizes the chemical reaction between oxygen-containing groups on the surface of graphene oxide and phosphate ions in the phosphate binder to introduce graphene oxide in situ into the phosphate molecular network structure, which not only effectively improves the compactness of the phosphate after curing, but also significantly improves the flexibility of the composite coating. The modified phosphate binder can be used as a high temperature resistant base resin binder, and has great application potential in the field of wide temperature range bonding solid lubricating coatings.

[0005] 1. Preparation of graphene oxide in-situ modified inorganic phosphate binder A preparation method for an inorganic phosphate binder modified by graphene oxide in situ comprises the following steps: firstly, 85% phosphoric acid and a graphene oxide dispersion treated by ultrasonic dispersion are mixed, mechanically stirred and heated to 130-150° C., then an alkaline oxide is slowly added to the mixture, and the mixture is stirred and refluxed for 2-6 hours and then naturally cooled to room temperature to obtain the inorganic phosphate binder modified by graphene oxide in situ.

[0006] The number of layers of the graphene oxide is 3 to 15, the ultrasonic dispersion treatment time is 30 to 50 min, and the addition amount is 0.1 to 5.0 wt% of the total mass of phosphoric acid.

[0007] The alkaline oxide is aluminum oxide or magnesium oxide, and the molar ratio of the alkaline oxide to phosphoric acid is (0.1-1.0):1.

[0008] 2. Preparation of wide temperature range bonded solid lubricating coating materials The inorganic phosphate binder modified in situ by graphene oxide is mixed with the lubricating filler and then sheared and dispersed on a high-speed shear disperser to obtain a wide temperature range bonding solid lubricating coating material.

[0009] The lubricating filler is a mixture of Ag powder and molybdenum disulfide, and the molar ratio of the two is (3-6):1.

[0010] The mass ratio of the graphene oxide in-situ modified inorganic phosphate binder to the lubricating filler is 1:(1-4).

[0011] The high-speed shear rate of the coating is 15000-20000 r / min, and the shear time is 1-8 min; the wide temperature range of the coating is 25-600°C.

[0012] 3. Performance of wide temperature range bonded solid lubricating coating The wide temperature range bonding solid lubricating coating material obtained by the present invention is applied to the surface of the part by a spray gun and cured at 120±10° C. for 2 hours. The temperature is then raised to 310±10° C. and cured for 1 hour before the mechanical properties and wide temperature range tribological properties are tested.

[0013] The specific test method is as follows: Adhesion: Test according to the method in GB / T1720 "Determination of paint film adhesion".

[0014] Flexibility: Tested in accordance with GB / T 1731-2020 "Determination of flexibility of paint films and putty films".

[0015] Impact resistance: Tested in accordance with GB / T 1732-2020 "Determination of impact resistance of paint films".

[0016] Tribological properties at different temperatures: The wide temperature range friction and wear properties of the coating were tested using a high temperature CSM friction tester. The test conditions were rotation mode, with a rotation radius of 0.5 cm, a linear speed of 5 cm / s, a load of 5 N, a Φ6 mm GCr15 steel ball as the dual ball, and the test temperatures were set at 25°C, 200°C, 400°C, 500°C and 600°C, respectively.

[0017] The test results show that the space lubrication protective coating material prepared by the present invention has an adhesion of level 0 on the metal substrate, a flexibility of 1 mm, an impact resistance of more than 50 cm, an average friction coefficient of the coating at 25°C, 200°C, 400°C, 500°C and 600°C is less than 0.25, and the wear life is greater than 30 min.

[0018] In summary, the present invention utilizes the chemical reaction between the oxygen-containing groups on the surface of graphene oxide and the phosphate ions to introduce graphene oxide in situ into the inorganic phosphate molecular network structure, which not only significantly improves the dispersion uniformity of graphene oxide in the phosphate binder, but also, due to the presence of multiple active reaction sites on the surface of graphene oxide, more phosphates are cross-linked by the bridging effect of graphene oxide to form a more compact POP spatial network structure, so that the lubricating filler in the composite coating is better wrapped by the phosphate binder, and finally the high temperature resistance of the lubricating coating is more excellent. In addition, due to the formation of a strong chemical bond between graphene oxide and the phosphoric acid molecule, the interface interaction between the two is stronger, and the introduction of graphene oxide at the molecular level reduces the overall regularity of the phosphate binder, improves the amorphous degree, and gives the lubricating coating excellent flexibility.

[0019] In addition, the preparation of the in-situ modified inorganic phosphate binder of graphene oxide provided by the present invention and its application in the bonding solid lubricating coating over a wide temperature range have simple binder modification and coating preparation processes, convenient construction, and are convenient for later industrial production and practical engineering applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a diagram of the internal microstructure of the wide temperature range bonding solid lubricating coating prepared in Example 1 of the present invention.

[0021] Figure 2 3 is the friction coefficient curve of the wide temperature range bonded solid lubricating coating prepared in Example 1 of the present invention at different temperatures. DETAILED DESCRIPTION

[0022] The technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work belong to the scope of protection of the present invention. The specific conditions and test methods not clearly described in the following embodiments are usually based on conventional conditions.

[0023] Example 1 Preparation of graphene oxide in-situ modified inorganic phosphate binder: Accurately weigh 70.0 g of 85% phosphoric acid in a three-necked flask. Disperse 0.6 g of graphene oxide in 30.0 g of deionized water, and then mix with the phosphoric acid in the three-necked flask after ultrasonic dispersion for 36 min. Heat the mixture to 138°C under mechanical stirring, and then slowly add 30.9 g of alumina powder to the mixture. Continue stirring and reflux reaction for 3 hours, and then naturally cool to room temperature to obtain a graphene oxide modified inorganic phosphate binder. Preparation of lubricating coating: Weigh 24.0 g of the modified inorganic phosphate binder and 50.0 g of mixed filler of Ag powder and molybdenum disulfide (wherein the molar ratio of Ag powder to molybdenum disulfide is 3:1), add deionized water to dilute to a total solid content of about 30%; then the mixed coating is sheared and dispersed on a high-speed shear disperser at 17000 r / min for 4 min to obtain a lubricating coating; finally, the dispersed lubricating coating is sprayed on the surface of tinplate and low-carbon steel substrates with compressed air or compressed nitrogen (the low-carbon steel surface is sandblasted before spraying, the tinplate is polished with 500-mesh sandpaper, and ultrasonically cleaned with acetone after sandblasting or sandpaper polishing). The coating thickness is controlled to be about 15 μm by controlling the number of spraying times. After the sprayed parts are placed in the air for 5-6 h, they are cured in a blast drying oven. The curing conditions are: 120±10℃ constant temperature for 2 h, then heated to 310±10℃ constant temperature for 1 h, and naturally cooled to room temperature.

[0024] The adhesion, flexibility and impact resistance of the coating were tested according to GB / T1720, GB / T 1731-2020 and GB / T 1732-2020 standards. The tribological properties of the coating were tested at 25°C, 200°C, 400°C, 500°C and 600°C using a CSM high temperature friction tester. The test results are shown in Table 1 and Appendix. Figure 2 shown.

[0025] Example 2 The preparation process of the in-situ modified inorganic phosphate binder with graphene oxide is the same as that in Example 1, except that the amount of graphene oxide added is increased from 0.6 g in Example 1 to 1.2 g, and other values ​​remain unchanged. The preparation and performance test of the lubricating coating are the same as those in Example 1, and the test results are listed in Table 1.

[0026] Example 3 The preparation process of the in-situ modified inorganic phosphate binder with graphene oxide is the same as that in Example 1, except that the aluminum oxide powder is replaced by magnesium oxide powder, and the amount of magnesium oxide powder added is 12.0 g, and other values ​​remain unchanged. The preparation and performance test of the lubricating coating are the same as those in Example 1, and the test results are listed in Table 1.

[0027] Example 4 The preparation process of the in-situ modified inorganic phosphate binder with graphene oxide is the same as that in Example 1, except that the amount of graphene oxide added is increased from 0.6 g in Example 1 to 1.2 g, and the aluminum oxide powder is replaced with magnesium oxide powder, the amount of magnesium oxide powder added is 12.0 g, and other values ​​remain unchanged. The preparation and performance test of the lubricating coating are the same as those in Example 1, and the test results are listed in Table 1.

[0028] Comparative Example 1 The preparation process of the in-situ modified inorganic phosphate binder with graphene oxide is the same as that in Example 1, except that 0.6 g of graphene oxide is removed and only 30.0 g of deionized water is added, and other values ​​remain unchanged. The preparation and performance test of the lubricating coating are the same as those in Example 1, and the test results are listed in Table 1.

[0029] Comparative Example 2 The preparation process of the in-situ modified inorganic phosphate binder with graphene oxide is the same as that in Example 1, except that 0.6 g of graphene oxide is removed and only 30.0 g of deionized water is added, and other values ​​remain unchanged. In the preparation process of the lubricating coating, 0.6 g of graphene oxide is added to the coating in the form of a filler, and other processes remain unchanged. The performance test of the coating is the same as that in Example 1, and the test results are listed in Table 1.

[0030] Table 1 Mechanical properties of the lubricating coatings prepared in various embodiments and comparative examples and the test results of tribological properties at different temperatures By comparing the mechanical properties of the lubricating coatings prepared in Examples 1 to 4 and Comparative Examples 1 to 2, it was found that the in-situ modification of the inorganic phosphate binder with graphene oxide can not only significantly improve the flexibility of the composite coating, but also significantly reduce the average friction coefficient of the composite coating, especially the friction coefficient at higher temperatures is more significantly reduced. This is mainly because the in-situ modification can ensure that the graphene oxide can be more evenly dispersed in the binder system, improve the amorphousness of the binder, and give the coating material good flexibility; at the same time, graphene oxide provides multiple reaction active points, and connects more phosphoric acid molecular networks through bridging action, thereby improving the density of the overall coating and improving the high-temperature lubrication performance. By comparing Examples 1 to 4, it is found that the in-situ introduction of different amounts of graphene oxide can improve the flexibility of the coating, and the inorganic magnesium phosphate and inorganic aluminum phosphate binders modified with graphene oxide both show good lubrication performance over a wide temperature range; compared with Comparative Example 1, it is found that the unmodified inorganic phosphate composite coating not only shows poor flexibility, but also has a large average friction coefficient over a wide temperature range; comparing the test results of each embodiment with Comparative Example 2, it is found that after graphene oxide is added to the coating system in the form of a blended filler, although the flexibility and the wide temperature range friction coefficient are improved to a certain extent, the modification effect is not obvious, which is mainly due to the limited dispersion uniformity, and its lubrication performance effect is far inferior to the in-situ modification technology.

Claims

1. A preparation method for in-situ modified inorganic phosphate binder by graphene oxide, characterized in that: 85% phosphoric acid and ultrasonically dispersed graphene oxide dispersion were mixed, mechanically stirred and heated to 130-150°C, and then alkaline oxide was slowly added to the mixture. After stirring and reflux reaction for 2-6 hours, the mixture was naturally cooled to room temperature to obtain the graphene oxide in-situ modified inorganic phosphate binder.

2. The preparation of a graphene oxide in-situ modified inorganic phosphate binder as claimed in claim 1, characterized in that: The number of layers of the graphene oxide is 3 to 15, the ultrasonic dispersion treatment time is 30 to 50 min, and the addition amount is 0.1 to 5.0 wt% of the total mass of phosphoric acid.

3. The preparation of a graphene oxide in-situ modified inorganic phosphate binder as claimed in claim 1, characterized in that: The alkaline oxide is aluminum oxide or magnesium oxide, and the molar ratio of the alkaline oxide to phosphoric acid is (0.1-1.0):

1.

4. An application of the in-situ modified inorganic phosphate binder of graphene oxide as claimed in claim 1 in bonding solid lubricating coatings over a wide temperature range.

5. The use of the in-situ modified inorganic phosphate binder of graphene oxide in bonding solid lubricating coatings over a wide temperature range as claimed in claim 4, characterized in that: The graphene oxide in-situ modified inorganic phosphate binder is mixed with the lubricating filler and then dispersed by high-speed shear to obtain a wide temperature range bonded solid lubricating coating material.

6. The use of the in-situ modified inorganic phosphate binder with graphene oxide as claimed in claim 5 in bonding solid lubricating coatings over a wide temperature range, characterized in that: The lubricating filler is a mixture of Ag powder and molybdenum disulfide, and the molar ratio of the two is (3-6):

1.

7. The use of the in-situ modified inorganic phosphate binder with graphene oxide as claimed in claim 5 in bonding solid lubricating coatings over a wide temperature range, characterized in that: The mass ratio of the graphene oxide in-situ modified inorganic phosphate binder to the lubricating filler is 1:(1-4).

8. The use of the in-situ modified inorganic phosphate binder with graphene oxide as claimed in claim 5 in bonding solid lubricating coatings over a wide temperature range, characterized in that: The high-speed shear rate is 15000-20000 r / min, and the shear time is 1-8 min.

9. The use of the in-situ modified inorganic phosphate binder with graphene oxide as claimed in claim 5 in bonding solid lubricating coatings over a wide temperature range, characterized in that: The coating has a wide temperature range of 25-600°C.

Citation Information

Patent Citations

  • Carbon fiber grafted graphene oxide modified phosphate bonding coating as well as preparation method and application thereof

    CN116855109A

Cited By

  • Composite nano coating on surface of diamond saw blade

    CN121182239A

  • A composite nano-coating for the surface of a diamond saw blade

    CN121182239B