Preparation method and application of core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material

By preparing the core sheath structure FeNi@(Co/CN)@ carbon fiber composite wave absorbing material on carbon fiber, the impedance mismatch and absorption of carbon fiber materials in electromagnetic wave absorption is solved by using coaxial electrospinning process and multi-heterogeneous interface design. The problem of narrow bandwidth achieves excellent microwave absorption performance.

CN118704120BActive Publication Date: 2024-11-05HEFEI INSTITUTE OF PHYSICAL SCIENCE CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411156855.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-05
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

Existing carbon fiber materials have impedance mismatch problems in electromagnetic wave absorption, resulting in insufficient absorption performance and insufficient magnetic loss resulting in a narrow effective absorption bandwidth.

Method used

The preparation method of the core sheath structure FeNi@(Co/CN)@@carbon fiber composite absorbing material is prepared by coaxial electrospinning process, and the FeNi@ZIF-67@polyacrylonitrile coaxial fiber is calcined at high temperature to form FeNi@ (Co/CN) structure, combining the dielectric loss of carbon fiber and the magnetic loss of FeNi and Co/CN, realizes the existence of multi-heterogeneous interfaces and the regulation of multi-components.

Benefits of technology

It achieves thin, light, wide and strong wave absorption performance in the frequency range of 2-18 GHz, showing a reflection loss of -61.84 dB and an effective absorption bandwidth of 6.24 GHz, improving the electromagnetic wave attenuation capability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118704120B_ABST
    Figure CN118704120B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of microwave absorbing materials, and specifically relates to a preparation method and application of a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material. The preparation method of the composite absorbing material of the present invention comprises: preparing ZIF-67 precursor powder, mixing a mixed solution containing polyacrylonitrile with ZIF-67 as an external phase solution, and mixing a mixed solution containing polyacrylonitrile with Fe powder and Ni powder as an internal phase solution; using a coaxial electrospinning process to manufacture coaxial fibers, and then placing them in a reducing atmosphere for carbonization to obtain a core-sheath structure FeNi@(Co / CN)@ carbon fiber. The prepared composite absorbing material is based on the advantages of core-sheath structure design, multi-heterogeneous interfaces and multi-components, realizes flexible microwave absorption performance regulation, has high absorption performance in a wide band range at low thickness, solves the problems of electromagnetic wave attenuation, insufficient magnetic loss and narrow effective absorption bandwidth existing in existing absorbing materials, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of microwave absorbing materials, and specifically designs a preparation method and application of a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material. Background Art

[0002] Carbon fiber is widely used in the military field due to its unique light weight and high strength. The high dielectric constant and single dielectric loss mechanism of carbon fiber usually lead to impedance mismatch. Existing technologies usually introduce other components inside or outside the carbon fiber to optimize impedance matching.

[0003] Metal organic frameworks (MOFs) have the advantages of light weight, rich topological structure, high specific surface area, adjustable pore structure, good compatibility and easy functionalization. MOFs derivatives obtained by high-temperature carbonization as precursors are evenly dispersed in carbon fibers to adjust the impedance mismatch problem of carbon fibers, which has been widely studied. However, a single component and limited heterogeneous interface cannot achieve flexible regulation, making it difficult to obtain effective electromagnetic wave attenuation, and insufficient magnetic loss leads to a narrow effective absorption bandwidth. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material. The preparation method effectively combines multiple loss mechanisms, especially the core-sheath structure design of the core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material and the advantages of multiple heterogeneous interfaces and multiple components, to obtain good impedance matching and achieve thin, light, wide and strong absorbing performance in the frequency range of 2-18 GHz, which is an ideal choice for new lightweight and efficient microwave absorbing materials.

[0005] To achieve the above object, the present invention adopts the following technical solution: a method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material, comprising the following steps:

[0006] Step S1, dissolving polyacrylonitrile in an organic solvent, mixing and stirring until clarified to obtain a mixed solution; taking part of the mixed solution as mixed solution 1, and mixing it evenly with ZIF-67 precursor powder with a particle size of 10-100 nm to serve as an external phase solution; taking part of the mixed solution as mixed solution 2, adding Fe powder and Ni powder, wherein the molar ratio of Fe powder to Ni powder is (1-3):(3-1), and mixing evenly to serve as an internal phase solution;

[0007] Step S2, using two syringes to draw the inner phase solution and the outer phase solution respectively, the injection is connected to a stainless steel needle, and the FeNi@ZIF-67@polyacrylonitrile coaxial fiber is prepared by a coaxial electrospinning process;

[0008] Step S3, placing the FeNi@ZIF-67@polyacrylonitrile coaxial fiber in a tube furnace, calcining it in a 5% (v / v) H2 / Ar mixed atmosphere at a temperature of 600-900°C for 1-5 h, and obtaining a core-sheath structure FeNi@(Co / CN)@carbon fiber composite absorbing material, wherein the composite absorbing material structurally includes carbon fiber and FeNi@(Co / CN) loaded in the carbon fiber, and the FeNi@(Co / CN) structure includes a FeNi alloy core layer and a Co / CN protective sheath coated on the surface of the core layer, and the Co / CN protective sheath is Co-loaded N-doped porous carbon.

[0009] Further improvement of the preparation method of FeNi@(Co / CN)@ carbon fiber composite absorber with core-sheath structure:

[0010] Preferably, a ZIF-67 precursor powder with a particle size of 10-100 nm is prepared by the following method: ultrasonically dissolving a metal cobalt salt in N,N-dimethylformamide to obtain a solution A; ultrasonically dissolving an organic ligand 2-methylimidazole in N,N-dimethylformamide to obtain a solution B; quickly mixing and stirring solution A and solution B, centrifuging the reaction mixture, washing and drying the separated solid, and obtaining a ZIF-67 precursor powder with a particle size of 10-100 nm.

[0011] Preferably, the molar concentration of the metal cobalt salt in solution A is 0.05-0.5 mol / L, the molar concentration of 2-methylimidazole in solution B is 0.5-1 mol / L, and when solution A and solution B are mixed, the molar ratio of the metal cobalt salt to 2-methylimidazole is 1:8.

[0012] Preferably, the metal cobalt salt is cobalt nitrate hexahydrate.

[0013] Preferably, the mixing and stirring of solution A and solution B is performed by magnetic stirring, the stirring speed is 500-1000 RPM, and the stirring time is 1-3 h; the speed of centrifugal separation of the reaction mixture is 8000-11000 RPM, and the centrifugation time is 10-30 min; the separated solid is washed and dried at 55-60° C. for 20-24 h.

[0014] Preferably, the organic solvent in step S1 is DMF, and the concentration of polyacrylonitrile in the mixed solution is 0.08-0.15 g / mL.

[0015] Preferably, in the external phase solution of step S1, the mass ratio of polyacrylonitrile in the mixed solution 1 to the ZIF-67 precursor powder is (1-4):1; in the internal phase solution of step S1, the ratio of polyacrylonitrile in the mixed solution 2 to the total mass of Fe powder and Ni powder is (1-4):1.

[0016] Preferably, in step S2, the parameters of the coaxial electrospinning process are as follows: receiving distance is 10-30 cm, propulsion rate is 0.05-0.2 mm / min, voltage is 10-20 kV, reciprocating translation distance is 80-120 mm, reciprocating translation rate is 400-600 mm / min, and drum speed is 100-200RPM.

[0017] Preferably, in step S3, the tube furnace is heated to the calcination temperature at a rate of 1-5°C / min.

[0018] Preferably, the second object of the present invention is to provide a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material obtained by the preparation method of the core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material described in any one of the above items and its application in the field of electromagnetic wave absorption.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1) The present invention provides a method for preparing a FeNi@(Co / CN)@ carbon fiber composite absorbing material, which adopts a coaxial electrospinning process. The coaxial electrospinning process can form a core-sheath structure of FeNi and Co / CN in the carbon fiber. The design of the core-sheath structure can effectively reduce the weight and obtain excellent absorbing performance at a thin thickness.

[0021] 2) The FeNi@(Co / CN)@ carbon fiber composite absorber prepared by the present invention comprises carbon fiber and FeNi@(Co / CN) loaded in the carbon fiber, wherein the FeNi@(Co / CN) structure comprises a FeNi core layer (FeNi alloy) and a Co / CN protective sheath (the product after carbonization of ZIF-67, i.e., a Co / CN composite, with a rhombic dodecahedron morphology) coated on the surface of the core layer. The presence of multiple heterogeneous interfaces is conducive to enhancing the interface polarization, promoting the dissipation and attenuation of electromagnetic waves inside the material, and obtaining satisfactory microwave absorption performance: it exhibits an impressive reflection loss (RL) of -61.84 dB with a thickness of 3.07 mm; in addition, when the thickness reaches 2.37 mm, the effective absorption bandwidth is extended to 6.24 GHz, which can be applied to the field of electromagnetic wave absorption.

[0022] 3) The electromagnetic wave absorption performance of the FeNi@(Co / CN)@ carbon fiber composite absorbing material prepared by the present invention is mainly derived from the dielectric loss of the carbon fiber itself and the magnetic loss caused by the FeNi and Co / CN loaded on the carbon fiber. By controlling the content and proportion of each component, the absorbing performance can be flexibly adjusted to achieve a balance in the impedance matching of the material and improve the electromagnetic wave attenuation capability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0024] Figure 1 A flow chart of preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material according to the present invention;

[0025] Figure 2 The three-dimensional graph of the minimum reflection loss of the product obtained at 700°C corresponding to different thicknesses of the Fe1Ni3@(Co / CN)@ carbon fiber composite absorbing material prepared in Example 1 of the present invention;

[0026] Figure 3 The scanning electron microscope images of the Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material prepared in Example 2 of the present invention, wherein the magnification of (a) is 3 KX, and the magnification of (b) is 10 KX;

[0027] Figure 4 The three-dimensional graph of the minimum reflection loss of the product obtained at 700°C corresponding to different thicknesses of the Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material prepared in Example 2 of the present invention;

[0028] Figure 5 The three-dimensional graph of the minimum reflection loss of the product obtained at 700°C corresponding to different thicknesses of the Fe3Ni1@(Co / CN)@ carbon fiber composite absorbing material prepared in Example 3 of the present invention;

[0029] Figure 6 The three-dimensional graph of the minimum reflection loss of the product obtained at 600°C corresponding to different thicknesses of the Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material prepared in Example 4 of the present invention;

[0030] Figure 7 This is a three-dimensional graph of the minimum reflection loss of the product obtained at 900°C corresponding to different thicknesses of the Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material prepared in Example 5 of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] This embodiment provides a method for preparing a Fe1Ni3@(Co / CN)@ carbon fiber composite absorbing material. The preparation process is as follows: Figure 1 As shown, the specific steps include:

[0034] Step S1, preparing ZIF-67 precursor powder

[0035] Co(NO3)2·6H2O was ultrasonically dissolved in N,N-dimethylformamide at a concentration of 0.1 mol / L to obtain solution A; 2-methylimidazole was ultrasonically dissolved in N,N-dimethylformamide at a concentration of 0.8 mol / L to obtain solution B; solution A and solution B were quickly mixed, wherein the molar ratio of Co(NO3)2·6H2O in solution A and 2-methylimidazole in solution B was 1:8; then stirred at 500 RPM for 2 h, and then centrifuged at 11000 RPM for 15 min, the separated solid was washed with N,N-dimethylformamide, and dried at 58 °C for 22 h to obtain ZIF-67 precursor powder with a particle size of 10-100 nm.

[0036] Step S2, preparing electrospinning solution

[0037] Dissolve 2.4 g of polyacrylonitrile in 20 mL of N,N-dimethylformamide, mix and stir until clear, and obtain a mixed solution with a concentration of 0.12 g / ml;

[0038] Take 10 mL of the mixed solution as mixed solution 1, add 0.6 g of the ZIF-67 precursor powder obtained in step S1, the mass ratio of polyacrylonitrile to ZIF-67 precursor powder in the mixed solution 1 is 2:1, and stir evenly at room temperature to prepare the external phase solution;

[0039] Take 10 mL of the mixed solution as mixed solution 2, add Fe powder and Ni powder, the mass ratio of polyacrylonitrile to Fe powder and Ni powder mixed powder in mixed solution 2 is 1:1, and the molar ratio of Fe powder to Ni powder is 1:3, and stir evenly at room temperature to prepare the internal phase solution.

[0040] Step S3, preparation of Fe1Ni3@ZIF-67@polyacrylonitrile coaxial fiber

[0041] Two 10 mL syringes were used to draw the inner phase solution and the outer phase solution respectively. The injection was connected to a stainless steel needle (medium size 22G / 17G). The Fe1Ni3@ZIF-67@polyacrylonitrile coaxial fiber was prepared by coaxial electrospinning process. The parameters of the coaxial electrospinning process were as follows: receiving distance was 15 cm, propulsion rate was 0.1 mm / min, voltage was 15 kV, reciprocating translation distance was 100 mm, reciprocating translation rate was 500 mm / min, and drum speed was 140 RPM.

[0042] Step S4, preparing Fe1Ni3@(Co / CN)@ carbon fiber composite absorbing material

[0043] The Fe1Ni3@ZIF-67@polyacrylonitrile coaxial fiber was placed in a tubular furnace and calcined at 700 ℃ at a rate of 3 ℃ / min in a 5% (v / v) H2 / Ar mixed atmosphere and maintained for 3 h to obtain a core-sheath structured Fe1Ni3@(Co / CN)@ carbon fiber composite absorbing material.

[0044] Figure 2 The three-dimensional graph of the minimum reflection loss of the Fe1Ni3@(Co / CN)@ carbon fiber composite absorbing material obtained in Example 1 of the present invention at 700°C corresponding to different thicknesses. Figure 2 It can be seen that when the matching thickness is 3.73 mm, the minimum reflection loss (RL min ) is -59.88 dB, and the effective absorption bandwidth (EAB) is 6.48 GHz when the matching thickness is 2.76 mm.

[0045] Example 2

[0046] This embodiment provides a method for preparing a Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material. The preparation process is as follows: Figure 1 As shown, the specific steps include:

[0047] Step S1, preparing ZIF-67 precursor powder

[0048] Co(NO3)2·6H2O was ultrasonically dissolved in N,N-dimethylformamide at a concentration of 0.1 mol / L to obtain solution A; 2-methylimidazole was ultrasonically dissolved in N,N-dimethylformamide at a concentration of 0.8 mol / L to obtain solution B; solution A and solution B were quickly mixed, wherein the molar ratio of Co(NO3)2·6H2O in solution A and 2-methylimidazole in solution B was 1:8; then stirred at 800 RPM for 1 h, and then centrifuged at 8000 RPM for 30 min, the separated solid was washed with N,N-dimethylformamide, and dried at 55 °C for 20 h to obtain a ZIF-67 precursor powder with a particle size of 10-100 nm.

[0049] Step S2, preparing electrospinning solution

[0050] Dissolve 2.4 g of polyacrylonitrile in 20 mL of N,N-dimethylformamide, mix and stir until clear, and obtain a mixed solution with a concentration of 0.12 g / ml;

[0051] Take 10 mL of the mixed solution as mixed solution 1, add 0.6 g of the ZIF-67 precursor powder obtained in step S1, the mass ratio of polyacrylonitrile to ZIF-67 precursor powder in the mixed solution 1 is 2:1, and stir evenly at room temperature to prepare the external phase solution;

[0052] Take 10 mL of the mixed solution as mixed solution 2, add Fe powder and Ni powder, the mass ratio of polyacrylonitrile to the mixed powder of Fe powder and Ni powder in mixed solution 2 is 1:1, and the molar ratio of Fe powder to Ni powder is 1:1, and stir evenly at room temperature to prepare the internal phase solution.

[0053] Step S3, preparation of Fe1Ni1@ZIF-67@polyacrylonitrile coaxial fiber

[0054] Two 10 mL syringes were used to draw the inner phase solution and the outer phase solution respectively. The injection was connected to a stainless steel needle (medium size 22G / 17G). The Fe1Ni1@ZIF-67@polyacrylonitrile coaxial fiber was prepared by coaxial electrospinning process. The parameters of the coaxial electrospinning process were as follows: receiving distance was 10 cm, propulsion rate was 0.05 mm / min, voltage was 10 kV, reciprocating translation distance was 80 mm, reciprocating translation rate was 400 mm / min, and drum speed was 100RPM.

[0055] Step S4, preparing Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material

[0056] The Fe1Ni1@ZIF-67@polyacrylonitrile coaxial fiber was placed in a tubular furnace and calcined at 700 ℃ in a 5% (v / v) H2 / Ar mixed atmosphere at a rate of 1 ℃ / min and maintained for 1 h to obtain a core-sheath structure Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material.

[0057] Figure 3 The scanning electron microscope images of the Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material prepared in Example 2 of the present invention at different magnifications; Figure 3 It can be seen that FeNi and Co / CN are evenly distributed on the carbon fiber.

[0058] Figure 4 The three-dimensional graph of the minimum reflection loss of the Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material obtained in Example 2 of the present invention at 700°C corresponding to different thicknesses. Figure 4 It can be seen that when the matching thickness is 3.07 mm, the minimum reflection loss (RLmin) is -61.84 dB, and when the matching thickness is 2.37 mm, the effective absorption bandwidth (EAB) is 6.24 GHz.

[0059] Example 3

[0060] This embodiment provides a method for preparing a Fe3Ni1@(Co / CN)@ carbon fiber composite absorbing material. The preparation process is as follows: Figure 1 As shown, the specific steps include:

[0061] Step S1, preparing ZIF-67 precursor powder

[0062] Co(NO3)2·6H2O was ultrasonically dissolved in N,N-dimethylformamide at a concentration of 0.1 mol / L to obtain solution A; 2-methylimidazole was ultrasonically dissolved in N,N-dimethylformamide at a concentration of 0.8 mol / L to obtain solution B; solution A and solution B were quickly mixed, wherein the molar ratio of Co(NO3)2·6H2O in solution A and 2-methylimidazole in solution B was 1:8; then stirred at 800 RPM for 3 h, and then centrifuged at 10000 RPM for 20 min, the separated solid was washed with N,N-dimethylformamide, and dried at 60 °C for 24 h to obtain ZIF-67 precursor powder with a particle size of 10-100 nm.

[0063] Step S2, preparing electrospinning solution

[0064] Dissolve 2.4 g of polyacrylonitrile in 20 mL of N,N-dimethylformamide, mix and stir until clear, and obtain a mixed solution with a concentration of 0.12 g / ml;

[0065] Take 10 mL of the mixed solution as mixed solution 1, add 0.6 g of the ZIF-67 precursor powder obtained in step S1, the mass ratio of polyacrylonitrile to ZIF-67 precursor powder in the mixed solution 1 is 2:1, and stir evenly at room temperature to prepare the external phase solution;

[0066] Take 10 mL of the mixed solution as mixed solution 2, add Fe powder and Ni powder, the mass ratio of polyacrylonitrile to Fe powder and Ni powder mixed powder in mixed solution 2 is 1:1, and the molar ratio of Fe powder to Ni powder is 3:1, and stir evenly at room temperature to prepare the internal phase solution.

[0067] Step S3, preparation of Fe3Ni1@ZIF-67@polyacrylonitrile coaxial fiber

[0068] Two 10 mL syringes were used to draw the inner phase solution and the outer phase solution respectively. The injection was connected to a stainless steel needle (medium size 22G / 17G). The Fe3Ni1@ZIF-67@polyacrylonitrile coaxial fiber was prepared by coaxial electrospinning process. The parameters of the coaxial electrospinning process were as follows: receiving distance was 30 cm; propulsion rate was 0.2 mm / min; voltage was 20 kV; reciprocating translation distance was 120 mm, reciprocating translation rate was 600 mm / min; drum speed was 200 RPM.

[0069] Step S4, preparing Fe3Ni1@(Co / CN)@ carbon fiber composite absorbing material

[0070] The Fe3Ni1@ZIF-67@polyacrylonitrile coaxial fiber was placed in a tubular furnace and calcined at 700 ℃ in a 5% (v / v) H2 / Ar mixed atmosphere at a rate of 5 ℃ / min and maintained for 5 h to obtain a core-sheath structured Fe3Ni1@(Co / CN)@ carbon fiber composite absorbing material.

[0071] Figure 5 The three-dimensional graph of the minimum reflection loss of the Fe3Ni1@(Co / CN)@ carbon fiber composite absorbing material obtained in Example 3 of the present invention at 700°C corresponding to different thicknesses. Figure 5 It can be seen that when the thickness is 4.17 mm, the minimum reflection loss (RL min ) is -54.87 dB, and the effective absorption bandwidth (EAB) is 5.55 GHz when the thickness is 2.52 mm.

[0072] Example 4

[0073] This embodiment provides a method for preparing a Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material. The preparation process is as follows: Figure 1 As shown, the specific steps include:

[0074] Step S1, preparing ZIF-67 precursor powder

[0075] Co(NO3)2·6H2O was ultrasonically dissolved in N,N-dimethylformamide at a concentration of 0.05 mol / L to obtain solution A; 2-methylimidazole was ultrasonically dissolved in N,N-dimethylformamide at a concentration of 0.5 mol / L to obtain solution B; solution A and solution B were quickly mixed, wherein the molar ratio of Co(NO3)2·6H2O in solution A and 2-methylimidazole in solution B was 1:8; then stirred at 1000 RPM for 1 h, and then centrifuged at 10000 RPM for 10 min, the separated solid was washed with N,N-dimethylformamide, and dried at 58 °C for 22 h to obtain ZIF-67 precursor powder with a particle size of 10-100 nm.

[0076] Step S2, preparing electrospinning solution

[0077] Dissolve 1.6 g of polyacrylonitrile in 20 mL of N,N-dimethylformamide, mix and stir until clear, and obtain a mixed solution with a concentration of 0.08 g / ml;

[0078] Take 10 mL of the mixed solution as mixed solution 1, add 0.8 g of the ZIF-67 precursor powder obtained in step S1, the mass ratio of polyacrylonitrile to ZIF-67 precursor powder in the mixed solution 1 is 1:1, and stir evenly at room temperature to prepare the external phase solution;

[0079] Take 10 mL of the mixed solution as mixed solution 2, add Fe powder and Ni powder, the mass ratio of polyacrylonitrile to Fe powder and Ni powder mixed powder in mixed solution 2 is 2:1, and the molar ratio of Fe powder to Ni powder is 1:1. Stir evenly at room temperature to prepare the internal phase solution.

[0080] Step S3, preparation of Fe1Ni1@ZIF-67@polyacrylonitrile coaxial fiber

[0081] Two 10 mL syringes were used to draw the inner phase solution and the outer phase solution respectively. The injection was connected to a stainless steel needle (medium size 22G / 17G). The Fe1Ni1@ZIF-67@polyacrylonitrile coaxial fiber was prepared by coaxial electrospinning process. The parameters of the coaxial electrospinning process were as follows: receiving distance was 20 cm, propulsion rate was 0.1 mm / min, voltage was 16 kV, reciprocating translation distance was 100 mm, reciprocating translation rate was 500 mm / min, and drum speed was 160 RPM.

[0082] Step S4, preparing Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material

[0083] The Fe1Ni1@ZIF-67@polyacrylonitrile coaxial fiber was placed in a tubular furnace and calcined at 600 ℃ at a rate of 3 ℃ / min in a 5% (v / v) H2 / Ar mixed atmosphere and maintained for 3 h to obtain a core-sheath structured Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material.

[0084] Figure 6 The three-dimensional graph of the minimum reflection loss of the Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material obtained in Example 4 of the present invention at 600°C corresponding to different thicknesses. Figure 6 It can be seen that when the matching thickness is 1.94 mm, the minimum reflection loss (RLmin) is -39.66 dB, and when the matching thickness is 2.4 mm, the effective absorption bandwidth (EAB) is 6.75 GHz.

[0085] Example 5

[0086] This embodiment provides a method for preparing a Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material. The preparation process is as follows: Figure 1 As shown, the specific steps include:

[0087] Step S1, preparing ZIF-67 precursor powder

[0088] Co(NO3)2·6H2O was ultrasonically dissolved in N,N-dimethylformamide at a concentration of 0.5 mol / L to obtain solution A; 2-methylimidazole was ultrasonically dissolved in N,N-dimethylformamide at a concentration of 1.0 mol / L to obtain solution B; solution A and solution B were quickly mixed, wherein the molar ratio of Co(NO3)2·6H2O in solution A and 2-methylimidazole in solution B was 1:8; then stirred at 600 RPM for 2 h, and then centrifuged at 11000 RPM for 15 min, the separated solid was washed with N,N-dimethylformamide, and dried at 55 °C for 21 h to obtain ZIF-67 precursor powder with a particle size of 10-100 nm.

[0089] Step S2, preparing electrospinning solution

[0090] Dissolve 3.0 g of polyacrylonitrile in 20 mL of N,N-dimethylformamide, mix and stir until clear, and obtain a mixed solution with a concentration of 0.15 g / ml;

[0091] Take 10 mL of the mixed solution as mixed solution 1, add 0.375 g of the ZIF-67 precursor powder obtained in step S1, the mass ratio of polyacrylonitrile to ZIF-67 precursor powder in the mixed solution 1 is 4:1, and stir evenly at room temperature as the external phase solution;

[0092] Take 10 mL of the mixed solution as mixed solution 2, add Fe powder and Ni powder, the mass ratio of polyacrylonitrile to Fe powder and Ni powder mixed powder in mixed solution 2 is 4:1, and the molar ratio of Fe powder to Ni powder is 1:1. Stir evenly at room temperature to prepare the internal phase solution.

[0093] Step S3, preparation of Fe1Ni1@ZIF-67@polyacrylonitrile coaxial fiber

[0094] Two 10 mL syringes were used to draw the inner phase solution and the outer phase solution respectively. The injection was connected to a stainless steel needle (medium size 22G / 17G). The Fe1Ni1@ZIF-67@polyacrylonitrile coaxial fiber was prepared by coaxial electrospinning process. The parameters of the coaxial electrospinning process were as follows: receiving distance was 20 cm, propulsion rate was 0.08 mm / min, voltage was 18 kV, reciprocating translation distance was 100 mm, reciprocating translation rate was 500 mm / min, and drum speed was 150 RPM.

[0095] Step S4, preparing Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material

[0096] The Fe1Ni1@ZIF-67@polyacrylonitrile coaxial fiber was placed in a tubular furnace and calcined at 900 ℃ in a 5% (v / v) H2 / Ar mixed atmosphere at a rate of 3 ℃ / min and maintained for 3 h to obtain a core-sheath structured Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material.

[0097] Figure 7 The three-dimensional graph of the minimum reflection loss of the Fe1Ni1@(Co / CN)@ carbon fiber composite absorbing material obtained in Example 5 of the present invention at 900°C corresponding to different thicknesses. Figure 7 It can be seen that when the matching thickness is 1.73 mm, the minimum reflection loss (RLmin) is -35.74 dB, and when the matching thickness is 2.07 mm, the effective absorption bandwidth (EAB) is 6.24 GHz.

[0098] Those skilled in the art should understand that the above are only some specific embodiments of the present invention, rather than all embodiments. It should be noted that for those of ordinary skill in the art, many modifications and improvements can be made, and all modifications or improvements that do not exceed the scope of protection of the present invention should be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material. It is characterized in that The steps include: Step S1, dissolving polyacrylonitrile in an organic solvent, mixing and stirring until clarified to obtain a mixed solution; A portion of the mixed solution is taken as mixed solution 1, and mixed evenly with ZIF-67 precursor powder with a particle size of 10-100 nm to serve as an external phase solution; Take part of the mixed solution as mixed solution 2, add Fe powder and Ni powder, wherein the molar ratio of Fe powder to Ni powder is (1-3):(3-1), mix well and form the internal phase solution; Step S2, using two syringes to draw the inner phase solution and the outer phase solution respectively, the injection is connected to a stainless steel needle, and the FeNi@ZIF-67@polyacrylonitrile coaxial fiber is prepared by a coaxial electrospinning process; Step S3: Place the FeNi@ZIF-67@polyacrylonitrile coaxial fiber in a tube furnace and heat it in 5% (v / v) H 2 / Ar mixed atmosphere and calcined at 600-900 ° C for 1-5 h to obtain a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material, which structurally includes carbon fiber and FeNi@(Co / CN) loaded in the carbon fiber, and the FeNi@(Co / CN) structure includes a FeNi alloy core layer and a Co / CN protective sheath coated on the surface of the core layer, and the Co / CN protective sheath is Co-loaded N-doped porous carbon.

2. The method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material according to claim 1, It is characterized in that The ZIF-67 precursor powder with a particle size of 10-100 nm is prepared by the following method: a metal cobalt salt is ultrasonically dissolved in N,N-dimethylformamide to obtain a solution A; an organic ligand 2-methylimidazole is ultrasonically dissolved in N,N-dimethylformamide to obtain a solution B; the solution A and the solution B are quickly mixed and stirred, the reaction mixture is centrifuged, and the separated solid is washed and dried to obtain a ZIF-67 precursor powder with a particle size of 10-100 nm.

3. The method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material according to claim 2, It is characterized in that The molar concentration of the metal cobalt salt in solution A is 0.05-0.5 mol / L, the molar concentration of 2-methylimidazole in solution B is 0.5-1 mol / L, and when solution A and solution B are mixed, the molar ratio of the metal cobalt salt to 2-methylimidazole is 1:

8.

4. A method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material according to claim 2 or 3, It is characterized in that The metal cobalt salt is cobalt nitrate hexahydrate.

5. The method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material according to claim 2, It is characterized in that The mixing and stirring method of solution A and solution B is magnetic stirring, the stirring speed is 500-1000 RPM, and the stirring time is 1-3 hours; the speed of centrifugal separation of the reaction mixture is 8000-11000 RPM, and the centrifugation time is 10-30 minutes; the separated solid is washed and dried at 55-60°C for 20-24 hours.

6. The method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material according to claim 1, It is characterized in that The organic solvent in step S1 is DMF, and the concentration of polyacrylonitrile in the mixed solution is 0.08-0.15 g / mL.

7. The method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material according to claim 1, It is characterized in that In the external phase solution of step S1, the mass ratio of polyacrylonitrile in the mixed solution 1 to the ZIF-67 precursor powder is (1-4):1; in the internal phase solution of step S1, the mass ratio of polyacrylonitrile in the mixed solution 2 to the total mass of Fe powder and Ni powder is (1-4):

1.

8. The method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material according to claim 1, It is characterized in that In step S2, the parameters of the coaxial electrospinning process are as follows: receiving distance is 10-30 cm, propulsion rate is 0.05-0.2 mm / min, voltage is 10-20 kV, reciprocating translation distance is 80-120 mm, reciprocating translation rate is 400-600 mm / min, and drum speed is 100-200 RPM.

9. The method for preparing a core-sheath structure FeNi@(Co / CN)@ carbon fiber composite absorbing material according to claim 1, It is characterized in that In step S3, the tube furnace is heated to the calcination temperature at a rate of 1-5°C / min.

10. Application of a core-sheath structure FeNi@(Co / CN)@carbon fiber composite absorbing material obtained by the method for preparing the core-sheath structure FeNi@(Co / CN)@carbon fiber composite absorbing material according to any one of claims 1 to 9 in the field of electromagnetic wave absorption.

Citation Information

Cited By

  • A magnetic manganese dioxide tunable electromagnetic wave absorbing material and its preparation method

    CN119551726B