A jade cool feeling anti-ultraviolet functional fabric and preparation method thereof
Through the blending and modification processing technology of knitted fabrics, the problems of poor moisture permeability and insufficient UV stability of knitted fabrics are solved, and the moisture permeability, coldness and easy-to-cleaning performance of the fabrics are coordinated and improved, and the product resistance is improved UV and water washing stability.
Patent Information
- Application Number
- CN202411178019.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing knitted fabrics have poor moisture permeability, are difficult to coordinate with the cool feeling, moisture permeability and oil-stained cleaning performance, and are insufficient in UV resistance and water washing stability, which limits the efficiency of the product.
The first blended yarn is formed by blending cotton fibers, spandex fibers and hemp fibers, and blended with modified polyester fibers. By mixing modified additives and ball mill additives, the impregnation and improvement treatment and heat setting technology of knitted fabric bodies are combined. Prepare a cool, UV-resistant functional fabric for jade.
It achieves coordinated improvements in moisture permeability, cold feeling and easy-to-clean performance of the fabric, and improves the UV resistance and washing stability of the product, and improves the use efficiency.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of knitted fabrics, and in particular to a jade-like cool-feeling anti-ultraviolet functional fabric and a preparation method thereof. Background Art
[0002] Knitted fabrics are soft, breathable, perspiration-wicking and warm, and most of them have excellent elasticity and extensibility. Compared with woven fabrics, they have high output and are suitable for small batch production. Knitted clothing is comfortable to wear, fits the body well, has no sense of tightness, and can fully reflect the curves of the human body.
[0003] Existing knitted fabrics have poor moisture permeability, and it is difficult to coordinate and improve the product's cooling feeling, moisture permeability, and oil-cleaning performance. At the same time, the product's UV resistance and water washing stability are poor, further limiting the product's use efficiency. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a jade cool anti-ultraviolet functional fabric and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution:
[0006] The present invention provides a method for preparing a jade-like cool anti-ultraviolet functional fabric, comprising the following steps:
[0007] Step 1: blending cotton fiber, spandex fiber and hemp fiber in a weight ratio of 2:2:1 in a carding process to form a first blended yarn, and then blending modal fiber and modified polyester fiber in a weight ratio of 1:1 in a carding process to form a second blended yarn;
[0008] Step 2, weaving the first blended yarn with a yarn count of 50S and the second blended yarn with a yarn count of 50S at a weight ratio of 4:3 using a knitting circular machine to obtain a knitted fabric body;
[0009] Step 3: the knitted fabric body is subjected to an impregnation improvement treatment, and after the treatment is completed, an impregnation improved fabric body is obtained;
[0010] Step 4, finally heat-setting the impregnated improved fabric body at 120° C. for 2-3 seconds, and the setting is completed to obtain a jade-like cool and UV-resistant functional fabric.
[0011] Preferably, the preparation method of the modified polyester fiber is:
[0012] S01: Preparation of modified additives:
[0013] S011: heat-treating the nano-bentonite at 230-240°C for 5-10 minutes, then cooling to 55°C at a rate of 1-3°C / min, and heat-treating to obtain heat-treated nano-bentonite;
[0014] S012: adding 1-2 parts of silane coupling agent KH560, 2-4 parts of sodium dodecylbenzene sulfonate and 0.4-0.7 parts of hydrochloric acid solution to 2-5 parts of chitosan solution and mixing thoroughly to obtain a modified solution;
[0015] S013: stirring the heat-treated nano-bentonite in a modification liquid of 4-7 times the total mass of the heat-treated nano-bentonite for modification, washing with water and drying after the stirring is completed to obtain modified nano-bentonite;
[0016] S014: The modified nano-bentonite and the ball milling additive are mixed and ball milled in a weight ratio of 5:2, the ball milling speed is 1000-1500r / min, the ball milling is performed for 2h, and after the ball milling is completed, the mixture is washed with water and dried to obtain a modified additive;
[0017] S02: mixing polyester resin, modified additives and jade powder with a particle size of 2µm in a weight ratio of 7:3:1, and then melt-blending and extruding to obtain an extrudate;
[0018] S03: The extrudate and the PBT polyester toughening agent are mixed at a weight ratio of 6:1, and then melt-spinned to obtain modified polyester fibers.
[0019] Preferably, the mass fraction of the chitosan solution is 4-6%; the mass fraction of the hydrochloric acid solution is 2-5%; the stirring speed of the stirring modification treatment is 450-550 r / min, and the stirring time is 30-40 min.
[0020] Preferably, the basic temperature of the melt blending extrusion is 285-300° C., and the extrusion pressure is 6-8 MPa; the spinning speed of the melt spinning is 2800-3200 m / min.
[0021] Preferably, the ball milling additive solution comprises the following raw materials in parts by weight:
[0022] 2-5 parts of nano silicon carbide, 3-6 parts of yttrium nitrate solution, 2-4 parts of sodium lignin sulfonate solution, 1-2 parts of citric acid and 2-3 parts of nano boron nitride.
[0023] Preferably, the mass fraction of the yttrium nitrate solution is 2-5%; the mass fraction of the sodium lignin sulfonate solution is 3-6%.
[0024] Preferably, the specific operation steps of the knitted fabric body impregnation improvement treatment are:
[0025] S11: irradiating the flake graphene in a proton irradiation box for 5-10 minutes at an irradiation power of 350-400 W, and obtaining irradiated flake graphene after the irradiation is completed;
[0026] S12: immersing the irradiated graphene flakes into a sufficient amount of phosphate buffer solution with a pH value of 5.5 and subjecting the solution to ultrasound at a power of 500 W and a time of 1-2 h to obtain a graphene flake solution;
[0027] 4-7 parts of flake graphene solution, 1-3 parts of lanthanum chloride solution, 2-5 parts of nano-silicon dioxide, 2-3 parts of glass fiber and 2-4 parts of silane coupling agent KH550 are mixed and ball-milled at a ball-milling speed of 1500 r / min for 2 hours to obtain an impregnation solution;
[0028] S13: Immerse the knitted fabric body in a sufficient amount of impregnation liquid for impregnation treatment, and after the impregnation is completed, take it out and dry it.
[0029] Preferably, the mass fraction of the lanthanum chloride solution is 2-5%.
[0030] Preferably, the immersion pressure of the immersion treatment is 15-20 MPa, and the immersion time is 1-2 h.
[0031] The present invention also provides a functional fabric prepared by a method for preparing the jade-like cool-feeling anti-ultraviolet functional fabric.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The functional fabric of the present invention adopts cotton fiber, spandex fiber and hemp fiber to form a first blended yarn, and then blends modal fiber and modified polyester fiber to form a second blended yarn. The modified polyester fiber adopts polyester resin, modified additive and jade powder with a particle size of 2μm as a base material, and the modified additive is used as a functional additive. The jade powder provides the cool feeling of jade. The modified additive adopts nano bentonite to be heat-treated at 230-240°C for 5-10min, and then at 1-3°C / The nano bentonite was cooled to 55°C at a rate of 100 min to optimize the active efficiency and interlayer spacing of the nano bentonite. At the same time, the modified solution obtained by blending chitosan solution, silane coupling agent KH560, sodium dodecylbenzene sulfonate and hydrochloric acid solution was used to improve the nano bentonite. The active dispersion of the improved nano bentonite was further improved, thereby further enhancing the synergistic effect of the nano bentonite and the ball milling additive. The ball milling additive adopts nano silicon carbide, yttrium nitrate solution, sodium lignin sulfonate solution, citric acid and nano nitride. Boron is blended and coordinated. Nano silicon carbide and nano boron nitride are used as the matrix materials, and yttrium nitrate solution, sodium lignin sulfonate solution and citric acid are coordinated to enhance the wetting and penetration improvement effect of the ball milling additive on nano bentonite. At the same time, the UV resistance and water washing stability of the product system are optimized. The modified polyester fiber is used as the matrix material to optimize the moisture permeability and cooling performance of the product. At the same time, the knitted fabric body is impregnated with the impregnation liquid to improve the knitted fabric body. The flake graphene liquid, lanthanum chloride solution and nano dioxygen in the impregnation liquid are impregnated with the impregnation liquid. Silicon dioxide, glass fiber and silane coupling agent KH550 are blended and ball-milled, and flaky graphene is used as a flaky structure to coordinate with nano-silicon dioxide and knitted glass fiber with a high specific surface area, so as to provide better cleaning points for the product system and optimize the easy-to-clean effect of the product. The modified polyester fiber of the present invention is coordinated with the impregnation liquid to impregnate the improved fabric body, and the two are coordinated and synergistic, so that the easy cleaning, cooling feeling and moisture permeability of the product can be coordinated and improved, and the UV resistance and water washing stability of the product are further improved. DETAILED DESCRIPTION
[0034] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The method for preparing a jade-like cool anti-ultraviolet functional fabric of the present embodiment comprises the following steps:
[0036] Step 1: blending cotton fiber, spandex fiber and hemp fiber in a weight ratio of 2:2:1 in a carding process to form a first blended yarn, and then blending modal fiber and modified polyester fiber in a weight ratio of 1:1 in a carding process to form a second blended yarn;
[0037] Step 2, weaving the first blended yarn with a yarn count of 50S and the second blended yarn with a yarn count of 50S at a weight ratio of 4:3 using a knitting circular machine to obtain a knitted fabric body;
[0038] Step 3: the knitted fabric body is subjected to an impregnation improvement treatment, and after the treatment is completed, an impregnation improved fabric body is obtained;
[0039] Step 4, finally heat-setting the impregnated improved fabric body at 120° C. for 2-3 seconds, and the setting is completed to obtain a jade-like cool and UV-resistant functional fabric.
[0040] The preparation method of the modified polyester fiber of this embodiment is:
[0041] S01: Preparation of modified additives:
[0042] S011: heat-treating the nano-bentonite at 230-240°C for 5-10 minutes, then cooling to 55°C at a rate of 1-3°C / min, and heat-treating to obtain heat-treated nano-bentonite;
[0043] S012: adding 1-2 parts of silane coupling agent KH560, 2-4 parts of sodium dodecylbenzene sulfonate and 0.4-0.7 parts of hydrochloric acid solution to 2-5 parts of chitosan solution and mixing thoroughly to obtain a modified solution;
[0044] S013: stirring the heat-treated nano-bentonite in a modification liquid of 4-7 times the total mass of the heat-treated nano-bentonite for modification, washing with water and drying after the stirring is completed to obtain modified nano-bentonite;
[0045] S014: The modified nano-bentonite and the ball milling additive are mixed and ball milled in a weight ratio of 5:2, the ball milling speed is 1000-1500r / min, the ball milling is performed for 2h, and after the ball milling is completed, the mixture is washed with water and dried to obtain a modified additive;
[0046] S02: mixing polyester resin, modified additives and jade powder with a particle size of 2µm in a weight ratio of 7:3:1, and then melt-blending and extruding to obtain an extrudate;
[0047] S03: The extrudate and the PBT polyester toughening agent are mixed at a weight ratio of 6:1, and then melt-spinned to obtain modified polyester fibers.
[0048] The mass fraction of the chitosan solution in this embodiment is 4-6%; the mass fraction of the hydrochloric acid solution is 2-5%; the stirring speed of the stirring modification treatment is 450-550 r / min, and the stirring time is 30-40 min.
[0049] The basic temperature of the melt blending extrusion in this embodiment is 285-300° C., and the extrusion pressure is 6-8 MPa; the spinning speed of the melt spinning is 2800-3200 m / min.
[0050] The ball milling additive solution of this embodiment includes the following raw materials in parts by weight:
[0051] 2-5 parts of nano silicon carbide, 3-6 parts of yttrium nitrate solution, 2-4 parts of sodium lignin sulfonate solution, 1-2 parts of citric acid and 2-3 parts of nano boron nitride.
[0052] The mass fraction of the yttrium nitrate solution in this embodiment is 2-5%; the mass fraction of the sodium lignin sulfonate solution is 3-6%.
[0053] The specific operation steps of the knitted fabric body impregnation improvement treatment of this embodiment are:
[0054] S11: irradiating the flake graphene in a proton irradiation box for 5-10 minutes at an irradiation power of 350-400 W, and obtaining irradiated flake graphene after the irradiation is completed;
[0055] S12: immersing the irradiated graphene flakes into a sufficient amount of phosphate buffer solution with a pH value of 5.5 and subjecting the solution to ultrasound at a power of 500 W and a time of 1-2 h to obtain a graphene flake solution;
[0056] 4-7 parts of flake graphene solution, 1-3 parts of lanthanum chloride solution, 2-5 parts of nano-silicon dioxide, 2-3 parts of glass fiber and 2-4 parts of silane coupling agent KH550 are mixed and ball-milled at a ball-milling speed of 1500 r / min for 2 hours to obtain an impregnation solution;
[0057] S13: Immerse the knitted fabric body in a sufficient amount of impregnation liquid for impregnation treatment, and after the impregnation is completed, take it out and dry it.
[0058] The mass fraction of the lanthanum chloride solution of the present embodiment is 2-5%.
[0059] The immersion pressure of the immersion treatment in this embodiment is 15-20 MPa, and the immersion time is 1-2 hours.
[0060] The present embodiment also provides a jade-like cool anti-ultraviolet functional fabric, which is prepared by the above-mentioned method for preparing the jade-like cool anti-ultraviolet functional fabric.
[0061] Embodiment 1: A method for preparing a jade cool anti-ultraviolet functional fabric, comprising the following steps:
[0062] Step 1: blending cotton fiber, spandex fiber and hemp fiber in a weight ratio of 2:2:1 in a carding process to form a first blended yarn, and then blending modal fiber and modified polyester fiber in a weight ratio of 1:1 in a carding process to form a second blended yarn;
[0063] Step 2, weaving the first blended yarn with a yarn count of 50S and the second blended yarn with a yarn count of 50S at a weight ratio of 4:3 using a knitting circular machine to obtain a knitted fabric body;
[0064] Step 3: the knitted fabric body is subjected to an impregnation improvement treatment, and after the treatment is completed, an impregnation improved fabric body is obtained;
[0065] Step 4, finally heat-setting the impregnated improved fabric body at 120° C. for 2 seconds, and the setting is completed to obtain a jade-like cool and UV-resistant functional fabric.
[0066] The preparation method of the modified polyester fiber of this embodiment is:
[0067] S01: Preparation of modified additives:
[0068] S011: heat-treating the nano-bentonite at 230°C for 5 minutes, cooling it to 55°C at a rate of 1°C / min, and heat-treating it to obtain heat-treated nano-bentonite;
[0069] S012: Add 1 part of silane coupling agent KH560, 2 parts of sodium dodecylbenzene sulfonate and 0.4 parts of hydrochloric acid solution to 2 parts of chitosan solution and mix thoroughly to obtain a modified solution;
[0070] S013: stirring the heat-treated nano-bentonite in a modification liquid of 4 times the total mass of the heat-treated nano-bentonite for modification, washing with water and drying after the stirring is completed to obtain modified nano-bentonite;
[0071] S014: The modified nano-bentonite and the ball milling additive solution are mixed and ball milled in a weight ratio of 5:2, the ball milling speed is 1000r / min, the ball milling is performed for 2h, and after the ball milling is completed, the mixture is washed with water and dried to obtain a modified additive;
[0072] S02: mixing polyester resin, modified additives and jade powder with a particle size of 2µm in a weight ratio of 7:3:1, and then melt-blending and extruding to obtain an extrudate;
[0073] S03: The extrudate and the PBT polyester toughening agent are mixed at a weight ratio of 6:1, and then melt-spinned to obtain modified polyester fibers.
[0074] The mass fraction of the chitosan solution in this embodiment is 4%; the mass fraction of the hydrochloric acid solution is 2%; the stirring speed of the stirring modification treatment is 450 r / min, and the stirring time is 30 min.
[0075] The basic temperature of the melt blending extrusion in this embodiment is 285° C., and the extrusion pressure is 6 MPa; the spinning speed of the melt spinning is 2800 m / min.
[0076] The ball milling additive solution of this embodiment includes the following raw materials in parts by weight:
[0077] 2 parts of nano silicon carbide, 3 parts of yttrium nitrate solution, 2 parts of sodium lignin sulfonate solution, 1 part of citric acid and 2 parts of nano boron nitride.
[0078] The mass fraction of the yttrium nitrate solution in this embodiment is 2%; the mass fraction of the sodium lignin sulfonate solution is 3%.
[0079] The specific operation steps of the knitted fabric body impregnation improvement treatment of this embodiment are:
[0080] S11: irradiating the graphene flakes in a proton irradiation box for 5 minutes at an irradiation power of 350 W, and obtaining irradiated graphene flakes after the irradiation is completed;
[0081] S12: immersing the irradiated graphene flakes into a sufficient amount of phosphate buffer solution with a pH value of 5.5 and subjecting the solution to ultrasound at a power of 500 W and a time of 1 h to obtain a graphene flake solution;
[0082] 4 parts of flake graphene solution, 1 part of lanthanum chloride solution, 2 parts of nano-silicon dioxide, 2 parts of glass fiber and 2 parts of silane coupling agent KH550 were mixed and ball-milled at a ball-milling speed of 1500 r / min for 2 hours to obtain an impregnation solution;
[0083] S13: Immerse the knitted fabric body in a sufficient amount of impregnation liquid for impregnation treatment, and after the impregnation is completed, take it out and dry it.
[0084] The mass fraction of the lanthanum chloride solution of the present embodiment is 2%.
[0085] The immersion pressure of the immersion treatment in this embodiment is 15 MPa, and the immersion time is 1 hour.
[0086] The present embodiment also provides a jade-like cool anti-ultraviolet functional fabric, which is prepared by the above-mentioned method for preparing the jade-like cool anti-ultraviolet functional fabric.
[0087] Embodiment 2: A method for preparing a jade cool anti-ultraviolet functional fabric, comprising the following steps:
[0088] Step 1: blending cotton fiber, spandex fiber and hemp fiber in a weight ratio of 2:2:1 in a carding process to form a first blended yarn, and then blending modal fiber and modified polyester fiber in a weight ratio of 1:1 in a carding process to form a second blended yarn;
[0089] Step 2, weaving the first blended yarn with a yarn count of 50S and the second blended yarn with a yarn count of 50S at a weight ratio of 4:3 using a knitting circular machine to obtain a knitted fabric body;
[0090] Step 3: the knitted fabric body is subjected to an impregnation improvement treatment, and after the treatment is completed, an impregnation improved fabric body is obtained;
[0091] Step 4, finally heat-setting the impregnated improved fabric body at 120° C. for 3 seconds, and the setting is completed to obtain a jade-like cool and UV-resistant functional fabric.
[0092] The preparation method of the modified polyester fiber of this embodiment is:
[0093] S01: Preparation of modified additives:
[0094] S011: heat-treating the nano-bentonite at 240°C for 10 minutes, cooling it to 55°C at a rate of 3°C / min, and heat-treating it to obtain heat-treated nano-bentonite;
[0095] S012: Add 2 parts of silane coupling agent KH560, 4 parts of sodium dodecylbenzene sulfonate and 0.7 parts of hydrochloric acid solution to 5 parts of chitosan solution and mix thoroughly to obtain a modified solution;
[0096] S013: stirring the heat-treated nano-bentonite in a modification liquid of 7 times the total mass of the heat-treated nano-bentonite for modification treatment, washing with water and drying after the stirring is completed to obtain modified nano-bentonite;
[0097] S014: The modified nano-bentonite and the ball milling additive solution are mixed and ball milled in a weight ratio of 5:2, the ball milling speed is 1500r / min, the ball milling is performed for 2h, and after the ball milling is completed, the mixture is washed with water and dried to obtain a modified additive;
[0098] S02: mixing polyester resin, modified additives and jade powder with a particle size of 2µm in a weight ratio of 7:3:1, and then melt-blending and extruding to obtain an extrudate;
[0099] S03: The extrudate and the PBT polyester toughening agent are mixed at a weight ratio of 6:1, and then melt-spinned to obtain modified polyester fibers.
[0100] The mass fraction of the chitosan solution in this embodiment is 6%; the mass fraction of the hydrochloric acid solution is 5%; the stirring speed of the stirring modification treatment is 550 r / min, and the stirring time is 40 min.
[0101] The basic temperature of the melt blending extrusion in this embodiment is 300° C., and the extrusion pressure is 8 MPa; the spinning speed of the melt spinning is 3200 m / min.
[0102] The ball milling additive solution of this embodiment includes the following raw materials in parts by weight:
[0103] 5 parts of nano silicon carbide, 6 parts of yttrium nitrate solution, 4 parts of sodium lignin sulfonate solution, 2 parts of citric acid and 3 parts of nano boron nitride.
[0104] The mass fraction of the yttrium nitrate solution in this embodiment is 5%; the mass fraction of the sodium lignin sulfonate solution is 6%.
[0105] The specific operation steps of the knitted fabric body impregnation improvement treatment of this embodiment are:
[0106] S11: irradiating the graphene flakes in a proton irradiation box for 10 minutes at an irradiation power of 400 W, and obtaining irradiated graphene flakes after the irradiation is completed;
[0107] S12: immersing the irradiated graphene flakes into a sufficient amount of phosphate buffer solution with a pH value of 5.5 and subjecting the solution to ultrasound at a power of 500 W and a time of 2 h to obtain a graphene flake solution;
[0108] 7 parts of flake graphene solution, 3 parts of lanthanum chloride solution, 5 parts of nano-silicon dioxide, 3 parts of glass fiber and 4 parts of silane coupling agent KH550 were mixed and ball-milled at a ball-milling speed of 1500 r / min for 2 hours to obtain an impregnation solution;
[0109] S13: Immerse the knitted fabric body in a sufficient amount of impregnation liquid for impregnation treatment, and after the impregnation is completed, take it out and dry it.
[0110] The mass fraction of the lanthanum chloride solution of the present embodiment is 5%.
[0111] The immersion pressure of the immersion treatment in this embodiment is 20 MPa, and the immersion time is 2 hours.
[0112] The present embodiment also provides a jade-like cool anti-ultraviolet functional fabric, which is prepared by the above-mentioned method for preparing the jade-like cool anti-ultraviolet functional fabric.
[0113] Embodiment 3: A method for preparing a jade cool anti-ultraviolet functional fabric, comprising the following steps:
[0114] Step 1: blending cotton fiber, spandex fiber and hemp fiber in a weight ratio of 2:2:1 in a carding process to form a first blended yarn, and then blending modal fiber and modified polyester fiber in a weight ratio of 1:1 in a carding process to form a second blended yarn;
[0115] Step 2, weaving the first blended yarn with a yarn count of 50S and the second blended yarn with a yarn count of 50S at a weight ratio of 4:3 using a knitting circular machine to obtain a knitted fabric body;
[0116] Step 3: the knitted fabric body is subjected to an impregnation improvement treatment, and after the treatment is completed, an impregnation improved fabric body is obtained;
[0117] Step 4, finally heat-setting the impregnated improved fabric body at 120° C. for 2.5 seconds, and the setting is completed to obtain a jade-like cool and UV-resistant functional fabric.
[0118] The preparation method of the modified polyester fiber of this embodiment is:
[0119] S01: Preparation of modified additives:
[0120] S011: heat-treating the nano-bentonite at 235°C for 7.5 minutes, then cooling to 55°C at a rate of 2°C / min, and heat-treating the nano-bentonite to obtain heat-treated nano-bentonite;
[0121] S012: adding 1.5 parts of silane coupling agent KH560, 3 parts of sodium dodecylbenzene sulfonate and 0.55 parts of hydrochloric acid solution to 3.5 parts of chitosan solution and mixing thoroughly to obtain a modified solution;
[0122] S013: stirring the heat-treated nano-bentonite in a modification liquid of 5.5 times the total mass of the heat-treated nano-bentonite for modification, washing with water and drying after the stirring is completed to obtain modified nano-bentonite;
[0123] S014: The modified nano-bentonite and the ball milling additive solution are mixed and ball milled in a weight ratio of 5:2, the ball milling speed is 1250r / min, the ball milling is performed for 2h, and after the ball milling is completed, the mixture is washed with water and dried to obtain a modified additive;
[0124] S02: mixing polyester resin, modified additives and jade powder with a particle size of 2µm in a weight ratio of 7:3:1, and then melt-blending and extruding to obtain an extrudate;
[0125] S03: The extrudate and the PBT polyester toughening agent are mixed at a weight ratio of 6:1, and then melt-spinned to obtain modified polyester fibers.
[0126] The mass fraction of the chitosan solution in this embodiment is 5%; the mass fraction of the hydrochloric acid solution is 3.5%; the stirring speed of the stirring modification treatment is 500 r / min, and the stirring time is 35 min.
[0127] The basic temperature of the melt blending extrusion in this embodiment is 288° C., and the extrusion pressure is 7 MPa; the spinning speed of the melt spinning is 3000 m / min.
[0128] The ball milling additive solution of this embodiment includes the following raw materials in parts by weight:
[0129] 3.5 parts of nano silicon carbide, 4.5 parts of yttrium nitrate solution, 3 parts of sodium lignin sulfonate solution, 1.5 parts of citric acid and 2.5 parts of nano boron nitride.
[0130] The mass fraction of the yttrium nitrate solution in this embodiment is 3.5%; the mass fraction of the sodium lignin sulfonate solution is 4.5%.
[0131] The specific operation steps of the knitted fabric body impregnation improvement treatment of this embodiment are:
[0132] S11: irradiating the graphene flakes in a proton irradiation box for 7.5 minutes at an irradiation power of 370 W, and obtaining irradiated graphene flakes after the irradiation is completed;
[0133] S12: immersing the irradiated graphene flakes into a sufficient amount of phosphate buffer solution with a pH value of 5.5 and subjecting the solution to ultrasound at a power of 500 W and a time of 1.5 h to obtain graphene flake liquid;
[0134] 5.5 parts of flake graphene solution, 2 parts of lanthanum chloride solution, 3.5 parts of nano-silicon dioxide, 2.5 parts of glass fiber and 3 parts of silane coupling agent KH550 were mixed and ball-milled at a ball-milling speed of 1500 r / min for 2 hours to obtain an impregnation solution;
[0135] S13: Immerse the knitted fabric body in a sufficient amount of impregnation liquid for impregnation treatment, and after the impregnation is completed, take it out and dry it.
[0136] The mass fraction of the lanthanum chloride solution of the present embodiment is 3.5%.
[0137] The immersion pressure of the immersion treatment in this embodiment is 17.5 MPa, and the immersion time is 1.5 h.
[0138] The present embodiment also provides a jade-like cool anti-ultraviolet functional fabric, which is prepared by the above-mentioned method for preparing the jade-like cool anti-ultraviolet functional fabric.
[0139] Comparative Example 1:
[0140] The difference from Example 3 is that the modified polyester fiber is replaced by polyester fiber.
[0141] Comparative Example 2:
[0142] The difference from Example 3 is that no modifying additive is added in the preparation of the modified polyester fiber.
[0143] Comparative Example 3:
[0144] The difference from Example 3 is that S011 treatment is not used in the modified additive.
[0145] Comparative Example 4:
[0146] The difference from Example 3 is that no modifying liquid treatment is used in the modifying additive.
[0147] Comparative Example 5:
[0148] The difference from Example 3 is that the modified additive is not treated with ball milling additive liquid.
[0149] Comparative Example 6:
[0150] The difference from Example 3 is that the knitted fabric body is not treated with dipping improvement.
[0151] Comparative Example 7:
[0152] The difference from Example 3 is that no flake graphene liquid is added to the impregnation liquid in the impregnation improvement treatment.
[0153] Comparative Example 8:
[0154] The difference from Example 3 is that nano silicon dioxide and glass fiber are not added to the impregnation solution.
[0155] Comparative Example 9:
[0156] The difference from Example 3 is that no lanthanum chloride solution and silane coupling agent KH550 are added to the impregnation solution.
[0157] The products of Examples 1 to 3 and Comparative Examples 1 to 9 were tested for moisture permeability (tested according to GB / T12704.1-2009 standard), cool contact coefficient (tested according to FZ / T62042-2020 standard), and degreasing grade (FZ / T4021-2011 standard). The tested products were then placed under 50mw / m 2 The product was irradiated under ultraviolet intensity for 10 hours and then washed with water 10 times to test its UV resistance and water washing stability. The test results are shown in Table 1.
[0158] Table 1: Product performance test results of Examples 1 to 3 and Comparative Examples 1 to 9
[0159]
[0160] It can be seen from Table 1 that the product of Example 3 has excellent water vapor permeability, and at the same time, excellent oil removal grade and cooling coefficient performance, and the three can be coordinated and improved. In addition, the product has significant effects on UV resistance and water washing condition stability;
[0161] From Comparative Examples 1 to 9 and Example 3, it can be seen that when the modified polyester fiber is replaced by the polyester fiber, the moisture permeability and cooling coefficient of the product have a significant deterioration trend, and the knitted fabric body is not treated by impregnation improvement, and the degreasing grade of the product has a significant deterioration trend; the modified polyester fiber is used in combination with the knitted fabric body to be treated by impregnation improvement, and the performance of the product can be improved in a coordinated manner;
[0162] In the preparation of the modified polyester fiber, no modification additive was added, S011 treatment was not used in the modification additive, modification liquid treatment was not used in the modification additive, ball milling additive treatment was not used in the modification additive, flake graphene liquid was not added to the impregnation liquid in the impregnation improvement treatment, nano-silicon dioxide and glass fiber were not added to the impregnation liquid, lanthanum chloride solution and silane coupling agent KH550 were not added to the impregnation liquid, and the performance of the product showed a trend of deterioration;
[0163] The modified polyester fiber obtained by using the modifying liquid of the present invention in combination with S011 treatment and ball milling additive liquid treatment has the most significant product performance effect. When the ball milling additive liquid is not used in the modification additive, the performance of the product shows a more obvious deterioration trend. The performance of the products obtained by different preparation methods of the impregnation liquid also shows different deterioration trends. Only when the specific impregnation liquid of the present invention is used for treatment, the performance effect of the product is the most obvious.
[0164] Based on the above tests, the present invention further explores the product performance by ball milling the additive liquid.
[0165] Experimental Example 1:
[0166] The only difference from Example 3 is that no nano-silicon carbide is added to the ball milling additive liquid.
[0167] Experimental Example 2:
[0168] The only difference from Example 3 is that no yttrium nitrate solution is added to the ball milling additive solution.
[0169] Experimental Example 3:
[0170] The only difference from Example 3 is that no sodium lignin sulfonate solution is added to the ball milling additive liquid.
[0171] Experimental Example 4:
[0172] The only difference from Example 3 is that no nano boron nitride is added to the ball milling additive solution.
[0173] Experimental Example 5:
[0174] The only difference from Example 3 is that no citric acid is added to the ball milling additive solution.
[0175] The same test was performed on the product performance of Experimental Examples 1-5, and the test results are shown in Table 2.
[0176] Table 2: Product performance test results of Experimental Examples 1-5
[0177]
[0178] As can be seen from Table 2, the performance of the product changes when no nano-silicon carbide and nano-boron nitride are added to the ball mill additive solution. In the composition of the ball mill additive solution, the performance deterioration is most obvious, especially the product under ultraviolet and water washing conditions, the performance stability deteriorates most obviously. At the same time, when no yttrium nitrate solution, sodium lignin sulfonate solution and citric acid are added to the ball mill additive solution, the performance of the product has a tendency to deteriorate. The performance of the product of the ball mill additive solution obtained by different combination ratios has a tendency to deteriorate to varying degrees. Only the ball mill additive solution obtained by the specific combination ratio of the present invention has the most significant product performance effect.
[0179] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0180] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a jade cool anti-ultraviolet functional fabric, characterized in that: The following steps are involved: Step 1: blending cotton fiber, spandex fiber and hemp fiber in a weight ratio of 2:2:1 in a carding process to form a first blended yarn, and then blending modal fiber and modified polyester fiber in a weight ratio of 1:1 in a carding process to form a second blended yarn; Step 2, weaving the first blended yarn with a yarn count of 50S and the second blended yarn with a yarn count of 50S at a weight ratio of 4:3 using a knitting circular machine to obtain a knitted fabric body; Step 3: the knitted fabric body is subjected to an impregnation improvement treatment, and after the treatment is completed, an impregnation improved fabric body is obtained; Step 4, finally heat setting the impregnated improved fabric body at 120° C. for 2-3 seconds, and the setting is completed to obtain a jade-like cool anti-ultraviolet functional fabric; The preparation method of the modified polyester fiber is: S01: Preparation of modified additives: S011: heat-treating the nano-bentonite at 230-240°C for 5-10 minutes, then cooling to 55°C at a rate of 1-3°C / min, and heat-treating to obtain heat-treated nano-bentonite; S012: adding 1-2 parts of silane coupling agent KH560, 2-4 parts of sodium dodecylbenzene sulfonate and 0.4-0.7 parts of hydrochloric acid solution to 2-5 parts of chitosan solution and mixing thoroughly to obtain a modified solution; S013: stirring the heat-treated nano-bentonite in a modification liquid of 4-7 times the total mass of the heat-treated nano-bentonite for modification, washing with water and drying after the stirring is completed to obtain modified nano-bentonite; S014: The modified nano-bentonite and the ball milling additive are mixed and ball milled in a weight ratio of 5:2, the ball milling speed is 1000-1500r / min, the ball milling is performed for 2h, and after the ball milling is completed, the mixture is washed with water and dried to obtain a modified additive; S02: mixing polyester resin, modified additives and jade powder with a particle size of 2µm in a weight ratio of 7:3:1, and then melt-blending and extruding to obtain an extrudate; S03: mixing the extrudate and the PBT polyester toughening agent in a weight ratio of 6:1, and then melt spinning to obtain modified polyester fibers; The mass fraction of the chitosan solution is 4-6%; the mass fraction of the hydrochloric acid solution is 2-5%; the stirring speed of the stirring modification treatment is 450-550r / min, and the stirring time is 30-40min; The basic temperature of the melt blending extrusion is 285-300°C, and the extrusion pressure is 6-8Mpa; the spinning speed of the melt spinning is 2800-3200m / min; The ball milling additive solution comprises the following raw materials in parts by weight: 2-5 parts of nano silicon carbide, 3-6 parts of yttrium nitrate solution, 2-4 parts of sodium lignin sulfonate solution, 1-2 parts of citric acid and 2-3 parts of nano boron nitride; The mass fraction of the yttrium nitrate solution is 2-5%; the mass fraction of the sodium lignin sulfonate solution is 3-6%.
2. The method for preparing a jade cool anti-ultraviolet functional fabric according to claim 1, characterized in that: The specific operation steps of the knitted fabric body impregnation improvement treatment are: S11: irradiating the flake graphene in a proton irradiation box for 5-10 minutes at an irradiation power of 350-400 W, and obtaining irradiated flake graphene after the irradiation is completed; S12: immersing the irradiated graphene flakes into a sufficient amount of phosphate buffer solution with a pH value of 5.5 and subjecting the solution to ultrasound at a power of 500 W and a time of 1-2 h to obtain a graphene flake solution; 4-7 parts of flake graphene solution, 1-3 parts of lanthanum chloride solution, 2-5 parts of nano-silicon dioxide, 2-3 parts of glass fiber and 2-4 parts of silane coupling agent KH550 are mixed and ball-milled at a ball-milling speed of 1500 r / min for 2 hours to obtain an impregnation solution; S13: Immerse the knitted fabric body in a sufficient amount of impregnation liquid for impregnation treatment, and after the impregnation is completed, take it out and dry it.
3. The method for preparing a jade cool anti-ultraviolet functional fabric according to claim 2, characterized in that: The mass fraction of the lanthanum chloride solution is 2-5%.
4. The method for preparing a jade cool anti-ultraviolet functional fabric according to claim 2, characterized in that: The immersion pressure of the immersion treatment is 15-20 MPa, and the immersion time is 1-2 hours.
5. A jade-like cool anti-ultraviolet functional fabric, prepared by the preparation method of a jade-like cool anti-ultraviolet functional fabric as described in any one of claims 1 to 4.