Electrode material for lithium-ion battery containing lithium iron phosphate and production method thereof

By forming a nitrogen-copper co-doped carbon composite cladding layer on the surface of the lithium iron phosphate electrode material, the problem of poor rate performance and cycle stability of the lithium iron phosphate electrode material is solved, and the diffusion rate and electrochemical performance of lithium ions are significantly improved, and the improvement of the improvement of the lithium ion is improved. The application range of lithium-ion batteries.

CN118712371BActive Publication Date: 2024-11-12RUICHI NEW ENERGY (XUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411181103.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The rate performance and cycle stability of lithium iron phosphate electrode materials are poor, which affects the application range of lithium-ion batteries.

Method used

By synthesizing lithium iron phosphate in situ in the cavity of the composite aerogel, and forming a nitrogen-copper co-doped carbon composite coating on the surface of the lithium iron phosphate, the xanthan gum and polyaniline complex is used to utilize electrostatic adsorption to complex the xanthan gum and polyaniline. Combined, a carbon film co-doped with nitrogen and copper is formed to uniformly wrap around the surface of lithium iron phosphate, improving conductivity and structural stability.

Benefits of technology

It effectively improves the diffusion rate of lithium ions and the electrochemical performance of electrode materials, enhances the rate performance and cycle stability, and significantly improves the electrochemical activity and conductivity of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118712371B_ABST
    Figure CN118712371B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrode materials, and discloses an electrode material for a lithium ion battery containing lithium iron phosphate and a production method thereof. The electrode material comprises the following raw materials: lithium iron phosphate material, acetylene black, polyvinylidene fluoride, and N-methylpyrrolidone; wherein the lithium iron phosphate material is prepared by in-situ synthesizing lithium iron phosphate in the cavity of a composite aerogel, and by controlling the particle size of the lithium iron phosphate to shorten the transmission path of lithium ions, thereby increasing the diffusion rate of lithium ions, and in the later sintering process, a nitrogen-copper co-doped carbon composite coating layer can be formed on the surface of the lithium iron phosphate, which is beneficial to maintaining the stability of the lithium iron phosphate structure, improving the conductivity of the lithium iron phosphate electrode material, so that the electrode material has good rate performance and cycle stability, and broadens the application range of lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrode materials, and in particular to an electrode material for a lithium ion battery containing lithium iron phosphate and a production method thereof. Background Art

[0002] Clean and efficient energy storage and conversion technology is an important pillar to promote the development of modern society. As one of the energy storage systems with the highest energy conversion efficiency, batteries have received more and more attention. Among the many battery systems, lithium-ion batteries have become the leader among batteries due to their high operating voltage, high specific energy, low self-discharge, good cycle performance, long service life, and light weight.

[0003] With the development of science and technology, the use of lithium-ion batteries is becoming more and more widespread, and the requirements for their technology are becoming higher and higher. As one of the core components of lithium-ion batteries, positive electrode materials play a key role in the comprehensive performance of lithium-ion batteries. The current commercial lithium battery positive electrode materials mainly include lithium cobalt oxide, lithium nickel oxide, ternary materials and lithium iron phosphate. Among them, lithium iron phosphate is widely used in lithium batteries due to its relatively high theoretical capacity, good thermal stability, high safety performance, no pollution to the environment, and long cycle life. However, lithium iron phosphate itself has some defects. Its special structure leads to a slow lithium ion diffusion rate and relatively low electronic conductivity, resulting in poor rate performance and cycle stability of the electrode material, which affects the application range of lithium-ion batteries. Therefore, it is of great significance to improve the rate performance and cycle stability of lithium iron phosphate electrode materials.

[0004] In the prior art, the performance of lithium iron phosphate electrode materials is improved mostly by coating, doping and other methods to improve the performance of lithium ion battery positive electrode materials. For example, the invention patent with publication number CN106025241B discloses a graphene aerogel-loaded lithium iron phosphate porous composite material and its preparation method. The invention prepares a graphene aerogel-loaded lithium iron phosphate porous composite material as a positive electrode material for lithium ion batteries, and improves the lithium ion diffusion performance of the material by controlling the particle size of lithium iron phosphate particles. At the same time, the excellent electrical conductivity of graphene significantly improves the electrical conductivity of the material. In addition, it has a porous three-dimensional structure, which can reduce the negative effects caused by volume expansion during charging and discharging, and improve the structural stability and cycle performance of the material. Based on this, the performance of lithium iron phosphate electrode materials can be improved by forming a carbon coating layer on the surface of lithium iron phosphate. Summary of the invention

[0005] The purpose of the present invention is to provide an electrode material for lithium ion batteries containing lithium iron phosphate and a production method thereof, which solves the following technical problems:

[0006] (1) Solved the problem of poor rate performance of lithium iron phosphate electrode materials;

[0007] (2) The problem of poor cycle stability of lithium iron phosphate electrode materials has been solved.

[0008] The purpose of the present invention can be achieved through the following technical solutions:

[0009] A method for producing an electrode material for a lithium ion battery containing lithium iron phosphate, comprising the following steps:

[0010] 70 to 90 parts by weight of lithium iron phosphate material, 15 to 25 parts of acetylene black and 10 to 20 parts of polyvinylidene fluoride are added to N-methylpyrrolidone solvent, stirred evenly at a rotation speed of 50 to 100 rpm, and prepared into a paste to obtain an electrode material.

[0011] Furthermore, the production method of the lithium iron phosphate material comprises the following steps:

[0012] AA1: Dissolve the iron source, phosphorus source and lithium source in deionized water, mix them evenly, and adjust the pH value to 7-8 with ammonia water to obtain a premixed solution;

[0013] AA2: ultrasonically disperse the composite aerogel in deionized water to form a dispersion, then add the premixed solution obtained in step AA1, ultrasonically disperse at an ultrasonic frequency of 60 to 80 kHz for 2 to 4 hours to obtain a mixed solution, and then transfer the mixed solution to an autoclave for hydrothermal reaction, introduce nitrogen protection, adjust the stirring speed in the autoclave to 500 to 700 rpm, adjust the temperature to 170 to 180° C., stir at a constant temperature for 5 to 10 hours, wash the product with distilled water for 3 to 5 times, and vacuum dry to obtain a lithium iron phosphate precursor;

[0014] AA3: Place the lithium iron phosphate precursor in a tubular furnace, and under argon protection, heat it from room temperature to 550-850°C at a heating rate of 5-15°C / min, keep it warm for 1-3 hours, and cool it to room temperature with the furnace to obtain lithium iron phosphate material.

[0015] Furthermore, in step AA1, the iron source is any one of ferrous chloride, ferric nitrate or ferrous oxalate; the phosphorus source is any one of sodium dihydrogen phosphate, ammonium phosphate or triethyl phosphate; and the lithium source is any one of lithium carbonate, lithium nitrate or lithium hydroxide.

[0016] Furthermore, the production method of the composite aerogel comprises the following steps:

[0017] Place xanthan gum in deionized water, stir evenly, add polyaniline complex, raise the temperature to 45-55°C after addition, keep stirring at this temperature for 5-7 hours, collect the product, and obtain composite aerogel by freeze-drying.

[0018] Furthermore, the freeze-drying process is as follows: the product is put into a mold, left to stand until it gels, and then the mold is stored at a temperature of -15 to -25°C for 4 to 8 hours, and then placed in a freeze dryer and freeze-dried at a temperature of -45 to -55°C for 12 to 24 hours.

[0019] Furthermore, the production method of the polyaniline complex comprises the following steps:

[0020] A1: Ultrasonic dispersion of polyaniline in dimethyl sulfoxide solution, adding bromoacetic acid and alkaline catalyst, mixing well, raising the system temperature to 50-60°C, stirring for 4-8 hours, and removing the solvent by rotary evaporation to obtain modified polyaniline;

[0021] A2: Add modified polyaniline and ethanol aqueous solution into a reaction kettle, stir evenly mechanically, then add copper salt, turn on the heating until the temperature in the reaction kettle reaches 50-70°C, stir and mix at a stirring rate of 100-300 r / min for 12-24 hours, wait for the material to cool naturally, discharge the material, and obtain a polyaniline complex.

[0022] Furthermore, in step A1, the alkaline catalyst is either sodium hydroxide or potassium hydroxide.

[0023] Furthermore, in step A2, the volume fraction of the ethanol aqueous solution is 40 to 80%.

[0024] Furthermore, in step A2, the copper salt is any one of copper acetate, copper sulfate pentahydrate, copper nitrate or copper chloride.

[0025] An electrode material for a lithium-ion battery containing lithium iron phosphate is produced by the production method.

[0026] Beneficial effects of the present invention:

[0027] (1) The present invention prepares lithium iron phosphate material by in-situ synthesizing lithium iron phosphate in the cavity of a composite aerogel, and then forming a nitrogen-copper co-doped carbon composite coating layer on the surface of the lithium iron phosphate through a sintering process. By synthesizing lithium iron phosphate in-situ in the cavity of the composite aerogel, the growth of grains can be prevented to a certain extent, the particle size of lithium iron phosphate can be controlled, the transmission path of lithium ions can be shortened, the diffusion rate of lithium ions can be increased, the diffusion impedance can be effectively reduced, and the rate performance of the electrode material can be improved, so that the battery exhibits excellent electrochemical performance. At the same time, coating the surface of lithium iron phosphate can inhibit the structural collapse and destruction of the electrode material during the charge and discharge process, which is beneficial to maintaining the stability of the lithium iron phosphate structure, so that the lithium ion battery exhibits good cycle stability.

[0028] (2) The present invention utilizes electrostatic adsorption to combine xanthan gum with a polyaniline complex to prepare a composite aerogel. In the subsequent sintering process, a nitrogen-copper co-doped carbon film can be formed to be uniformly wrapped on the surface of lithium iron phosphate. On the one hand, the copper-carbon composite wrapping layer can effectively improve the conductivity of the lithium iron phosphate electrode material, improve the rate capability of the lithium iron phosphate electrode material, and improve the electrochemical performance of the material. On the other hand, doping nitrogen into the carbon material can introduce a rich defect structure, so that the carbon material has stronger electrochemical activity such as conductivity. At the same time, it can also improve the wettability of the carbon material, which is conducive to the rapid penetration of the electrolyte, accelerate the transfer of ions and electrons, and further improve the electrochemical activity of the electrode material.

[0029] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0031] Figure 1 This is an infrared spectrum test chart of the modified polyaniline prepared in the present invention.

[0032] Figure 2 This is a scanning electron microscope image of the composite aerogel prepared in the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The lithium iron phosphate material in the embodiment of the present invention is prepared by the following method:

[0035] Step 1: Preparation of polyaniline complex

[0036] A1: 5 g of polyaniline was ultrasonically dispersed in a dimethyl sulfoxide solution, 1.4 g of bromoacetic acid and 0.1 g of sodium hydroxide were added, and the mixture was mixed. The system temperature was raised to 55°C, and the mixture was stirred for 6 h. The solvent was removed by rotary evaporation to obtain modified polyaniline.

[0037] The modified polyaniline was analyzed by infrared spectroscopy using the IR2000 spectrometer produced by Thermo Electron Company of the United States. The analysis results are shown in Figure 1 ,Depend on Figure 1 It can be seen that in the infrared spectrum of modified polyaniline, 3030cm -1 The absorption peak of CH in the benzene ring appears at 3421cm -1 The absorption peak of NH appears at 1758 cm -1 The absorption peak of C=O in the carboxyl group appears at 1331 cm -1 The absorption peak of CN appears at

[0038] A2: Add 5 g of modified polyaniline and 50% ethanol aqueous solution in a reaction kettle, stir mechanically to make them uniform, then add 2.2 g of copper sulfate pentahydrate. After the addition, turn on the heating until the temperature in the reaction kettle reaches 60°C, stir and mix at a stirring rate of 200 r / min for 18 hours, wait for the material to cool naturally, discharge the material, and obtain a polyaniline complex;

[0039] The copper content in the polyaniline complex was tested using SpectrA A220FS atomic absorption spectrometer (AAS). The test showed that the mass fraction of copper in the prepared polyaniline complex was 4.81%.

[0040] It can be inferred that the principle of the above scheme is: the polyaniline structure contains an imino group, which can react with the halogen functional group in the bromoacetic acid structure under the action of sodium hydroxide, thereby introducing a carboxyl group into the structure of the polyaniline to obtain modified polyaniline. In an ethanol aqueous solution, the carboxyl group in the polyaniline structure can react with the copper ions in the copper sulfate pentahydrate structure to complex the divalent copper ions in the polyaniline structure to obtain a polyaniline complex.

[0041] Step 2: Preparation of composite aerogel

[0042] 15g of xanthan gum was placed in deionized water and stirred evenly. 2.8g of polyaniline complex was added. After the addition, the temperature was raised to 50°C. The mixture was stirred for 6 hours under the temperature condition. The product was collected and put into a mold. The mold was placed at -20°C for storage for 6 hours. The mold was placed in a freeze dryer and freeze-dried at -50°C for 18 hours. The composite aerogel was obtained.

[0043] The composite aerogel was analyzed using a Hitachi S-4700 scanning electron microscope. The test results are shown in Figure 2 As can be observed from the figure, the composite aerogel presents a porous surface morphology. These porous structures are conducive to the flow of phosphorus, iron, and lithium into the pores of the aerogel and the formation of lithium iron phosphate in the cavity of the composite aerogel.

[0044] It can be inferred that the principle of the above scheme is: to utilize the negative charge of xanthan gum in the solution to undergo electrostatic adsorption with the positively charged polyaniline main chain, thereby tightly combining the xanthan gum and polyaniline complex, and then through a freeze-drying process, a composite aerogel can be obtained.

[0045] Step 3: Preparation of lithium iron phosphate material

[0046] AA1: Dissolve 0.3 g of ferrous chloride, 0.04 g of sodium dihydrogen phosphate, and 0.008 g of lithium carbonate in deionized water, mix evenly, and adjust the pH value to 7.5 with ammonia water to obtain a premixed solution;

[0047] AA2: Ultrasonic dispersion of 2 g of the composite aerogel in deionized water to form a dispersion, and then adding the premixed solution obtained in step AA1, ultrasonic dispersion at an ultrasonic frequency of 70 KHz for 3 h to obtain a mixed solution, and then transferring the mixed solution to an autoclave for hydrothermal reaction, introducing nitrogen protection, adjusting the stirring speed in the autoclave to 600 rpm, adjusting the temperature to 175 ° C, and stirring at a constant temperature for 8 h. The product was washed 4 times with distilled water and vacuum dried to obtain a lithium iron phosphate precursor;

[0048] AA3: The lithium iron phosphate precursor was placed in a tubular furnace, and heated from room temperature to 700°C at a heating rate of 10°C / min under argon protection, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain the lithium iron phosphate material.

[0049] It can be inferred that the principle of the above scheme is: using composite aerogel as the matrix for the synthesis of lithium iron phosphate, under ultrasonic conditions, phosphorus, iron, and lithium will flow into the pores of the composite aerogel and form lithium iron phosphate in the cavity of the composite aerogel, and then through high-temperature treatment, a nitrogen-copper co-doped carbon composite coating layer is formed on the surface of the lithium iron phosphate.

[0050] Example 1

[0051] Preparation of electrode materials

[0052] 70 g of lithium iron phosphate material, 15 g of acetylene black and 10 g of polyvinylidene fluoride were added to N-methylpyrrolidone solvent, stirred evenly at a rotation speed of 50 rpm, and prepared into a paste to obtain an electrode material.

[0053] Example 2

[0054] Preparation of electrode materials

[0055] 80 g of lithium iron phosphate material, 20 g of acetylene black and 15 g of polyvinylidene fluoride were added to N-methylpyrrolidone solvent, stirred evenly at a rotation speed of 80 rpm, and prepared into a paste to obtain an electrode material.

[0056] Example 3

[0057] Preparation of electrode materials

[0058] 90 g of lithium iron phosphate material, 25 g of acetylene black and 20 g of polyvinylidene fluoride were added to N-methylpyrrolidone solvent, stirred evenly at a rotation speed of 100 rpm, and prepared into a paste to obtain an electrode material.

[0059] Comparative Example 1

[0060] Preparation of electrode materials

[0061] 80 g of commercially available lithium iron phosphate, 20 g of acetylene black and 15 g of polyvinylidene fluoride were added to N-methylpyrrolidone solvent, stirred evenly at a rotation speed of 80 rpm, and prepared into a paste to obtain an electrode material.

[0062] Note: Commercially available lithium iron phosphate was purchased from Hubei Xinyuhong Biomedicine Technology Co., Ltd.

[0063] Performance testing:

[0064] ① The electrode materials prepared in Examples 1 to 3 and Comparative Example 1 were uniformly coated on the surface of aluminum foil, placed in a vacuum drying oven at 100°C for 10 hours, and then the aluminum foil was made into a positive electrode sheet with a diameter of 10 mm, a metal lithium sheet was used as a counter electrode, and the electrolyte was 1 mon / L LiPF6. The positive electrode sheet, the electrolyte, the PP diaphragm and the metal lithium sheet were assembled into a conventional battery in a glove box protected by pure argon gas using a shell of model CR2032 to obtain a lithium battery. After standing in a constant temperature box at 25°C for 24 hours, the positive electrode of the assembled lithium battery was tested by cyclic voltammetry using a CH1600D electrochemical workstation to calculate the capacity retention rate. The specific test results are shown in the following table:

[0065] Table 1 - Capacity retention rate test results

[0066]

[0067] From the test results in Table 1, it can be seen that the lithium batteries prepared in Examples 1 to 3 have good rate performance and cycle stability; the lithium battery prepared in Comparative Example 1 has a low discharge specific capacity at 1C rate, 3C rate, and 10C rate. After 50 cycles at 10C rate, the capacity retention rate is less than 90%. Compared with the embodiments, the rate performance and cycle stability of the lithium battery are poor, which may be because no coating layer is formed on the surface of lithium iron phosphate, the electrical conductivity of the electrode material is low, and the diffusion rate of lithium ions is slow, resulting in poor rate performance and cycle stability of the lithium battery.

[0068] ② The electrode materials prepared in Examples 1 to 3 and Comparative Example 1 were ground with agate, passed through a 300-mesh sieve, and then tested for resistivity using a FT-354 powder resistivity tester. The specific test results are shown in the following table:

[0069] Table 2 - Resistivity test results

[0070]

[0071] From the test results in Table 2, it can be seen that the electrode materials prepared in Examples 1 to 3 have low resistivity and excellent conductive properties; the electrode material prepared in Comparative Example 1 does not form a nitrogen-copper co-doped carbon composite coating layer on the surface of the lithium iron phosphate, and compared with the examples, has a higher resistivity, so the conductive properties are poor.

[0072] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for producing an electrode material for a lithium ion battery containing lithium iron phosphate, characterized in that: The following steps are involved: Add 70 to 90 parts by weight of lithium iron phosphate material, 15 to 25 parts of acetylene black and 10 to 20 parts of polyvinylidene fluoride into N-methylpyrrolidone solvent, stir evenly at a speed of 50 to 100 rpm to prepare a paste to obtain an electrode material; The production method of the lithium iron phosphate material comprises the following steps: AA1: Dissolve the iron source, phosphorus source and lithium source in deionized water, mix them evenly, and adjust the pH value to 7-8 with ammonia water to obtain a premixed solution; AA2: ultrasonically disperse the composite aerogel in deionized water to form a dispersion, then add the premixed solution obtained in step AA1, ultrasonically disperse at an ultrasonic frequency of 60 to 80 kHz for 2 to 4 hours to obtain a mixed solution, and then transfer the mixed solution to an autoclave for hydrothermal reaction, introduce nitrogen protection, adjust the stirring speed in the autoclave to 500 to 700 rpm, adjust the temperature to 170 to 180° C., stir at a constant temperature for 5 to 10 hours, wash the product with distilled water for 3 to 5 times, and vacuum dry to obtain a lithium iron phosphate precursor; AA3: Place the lithium iron phosphate precursor in a tubular furnace, and heat it from room temperature to 550-850°C at a heating rate of 5-15°C / min under argon protection, keep it warm for 1-3 hours, and cool it to room temperature with the furnace to obtain the lithium iron phosphate material; The production method of the composite aerogel comprises the following steps: Place xanthan gum in deionized water, stir evenly, add polyaniline complex, raise the temperature to 45-55°C after adding, keep stirring at this temperature for 5-7h, collect the product, and freeze-dry to obtain composite aerogel; The production method of the polyaniline complex comprises the following steps: A1: Ultrasonic dispersion of polyaniline in dimethyl sulfoxide solution, adding bromoacetic acid and alkaline catalyst, mixing well, raising the system temperature to 50-60°C, stirring for 4-8 hours, and removing the solvent by rotary evaporation to obtain modified polyaniline; A2: Add modified polyaniline and ethanol aqueous solution into a reaction kettle, stir evenly mechanically, then add copper salt, turn on the heating until the temperature in the reaction kettle reaches 50-70°C, stir and mix at a stirring rate of 100-300 r / min for 12-24 hours, wait for the material to cool naturally, discharge the material, and obtain a polyaniline complex.

2. The method for producing an electrode material for a lithium ion battery containing lithium iron phosphate according to claim 1, characterized in that: In step AA1, the iron source is any one of ferrous chloride, ferric nitrate or ferrous oxalate; the phosphorus source is any one of sodium dihydrogen phosphate, ammonium phosphate or triethyl phosphate; and the lithium source is any one of lithium carbonate, lithium nitrate or lithium hydroxide.

3. The method for producing an electrode material for a lithium ion battery containing lithium iron phosphate according to claim 1, characterized in that: The freeze-drying process is as follows: the product is put into a mold, left to stand until it gels, and then the mold is stored at a temperature of -15 to -25°C for 4 to 8 hours, and then placed in a freeze dryer for freeze drying at a temperature of -45 to -55°C for 12 to 24 hours.

4. The method for producing an electrode material for a lithium ion battery containing lithium iron phosphate according to claim 1, characterized in that: In step A1, the alkaline catalyst is either sodium hydroxide or potassium hydroxide.

5. The method for producing an electrode material for a lithium ion battery containing lithium iron phosphate according to claim 1, characterized in that: In step A2, the volume fraction of the ethanol aqueous solution is 40-80%.

6. The method for producing an electrode material for a lithium ion battery containing lithium iron phosphate according to claim 1, characterized in that: In step A2, the copper salt is any one of copper acetate, copper sulfate pentahydrate, copper nitrate or copper chloride.

7. An electrode material for a lithium ion battery containing lithium iron phosphate, characterized in that: The method is produced according to claim 1.