Plantain seed polysaccharide-nano-selenium compound as well as preparation method and application thereof

By using Plantago polysaccharide as a dispersant and stabilizer in the preparation of nano-selenium and using redox reactions to prepare nano-selenium, the problems of agglomeration and insufficient biological activity of nano-selenium particles are solved, and small particle size, high stability and high stability are achieved. Psyllium polysaccharide-nano selenium complex with antioxidant activity is suitable for antioxidant drugs and health products.

CN118716625AInactive Publication Date: 2024-10-01NANCHANG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410734871.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to control the morphology and functional properties of nano-selenium particles using existing nano-selenium preparation methods, and selenium elements easily aggregate and precipitate during chemical synthesis, affecting their particle size, bioavailability and biological activity.

Method used

Plantago polysaccharide is used as a dispersant and stabilizer, and nano-selenium is prepared in a water extraction and alcohol precipitation method through a redox reaction. Sodium selenite is used as an oxidant and ascorbic acid is used as a reducing agent to prevent the agglomeration of nano-selenium particles and the formation of small particle sizes. , spherical nano-selenium particles with high stability.

Benefits of technology

The prepared Plantago polysaccharide-nano-selenium has high antioxidant activity, can effectively scavenge DPPH, ABTS and hydroxyl radicals, significantly improve the biological activity of nano-selenium, and the preparation method is simple, green and safe, and the product contains high selenium content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118716625A_ABST
    Figure CN118716625A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of food processing, and particularly relates to a semen plantaginis polysaccharide-nano-selenium compound as well as a preparation method and application thereof. The method comprises the following steps: performing boiling water extraction, alcohol precipitation, deproteinization, concentration and freeze-drying on semen plantaginis powder to obtain semen plantaginis polysaccharide; the preparation method comprises the following steps: dissolving semen plantaginis polysaccharide in water to obtain a semen plantaginis polysaccharide solution, adding a sodium selenite solution, mixing, dropwise adding an ascorbic acid solution, reacting in a constant-temperature water bath, and dialyzing and freeze-drying after the reaction is finished to finally obtain the semen plantaginis polysaccharide-nano-selenium. The semen plantaginis polysaccharide-nano-selenium compound which is small in particle size, high in electrostatic stability and higher in antioxidant activity is prepared. The preparation method is simple and easy to operate and short in time consumption, a reaction system does not involve strong acid and alkali chemical reagents and is green and safe, the selenium content of the product is high, and the system is stable; the invention provides a theoretical basis for research and development of plantain seed polysaccharide-nano-selenium and selenium-rich functional foods, and provides a theoretical basis for development of novel health foods and medicines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of food processing, and in particular relates to a psyllium polysaccharide-nano selenium complex and a preparation method and application thereof. Background Art

[0002] Selenium is a metalloid trace element that is essential for maintaining human health. It cannot be synthesized in the human body and is one of the 14 essential trace elements for the human body. Since selenium cannot be synthesized in the body and must be taken from food, selenium deficiency in the human body is very common. When the human body is deficient in selenium, it mainly affects the normal physiological state of bones and cartilage through oxidative stress response and immune response, thereby causing joint diseases such as Kashin-Beck disease, osteoarthritis and osteoporosis. The concentration range between selenium deficiency and selenium excess is narrow. Excessive selenium supplementation will cause certain toxic effects on human growth and development, and in severe cases, it may even lead to death.

[0003] With the development of new nanotechnology, nano-selenium particles have become a promising biomedical agent due to their low toxicity, degradability and high bioavailability. People usually use macromolecules as stabilizers or dispersants to prepare stable nano-selenium materials. Polysaccharides, as biomacromolecules, have low toxicity and diverse biological activities, such as anti-inflammatory, anti-tumor, anti-viral, antioxidant, immunomodulatory, hypoglycemic, and hypolipidemic. Among them, plant polysaccharides have the advantages of biodegradability, easy modification, low immunogenicity and low toxicity. They can be coupled, cross-linked or functionally modified with nanomaterials to play an effective therapeutic role. Studies have shown that polysaccharide-nanoselenium has biological activities such as antioxidant, anti-tumor, improving immunity, hypoglycemic, hypolipidemic, anti-heavy metal, and antibacterial and anti-inflammatory. In addition, red amorphous elemental selenium with a particle size of less than 100 nm has higher antioxidant activity and lower toxicity than general selenium. The prior art has found that spherical nano-selenium particles modified with chitosan of different molecular weights have good scavenging ability for free radicals such as DPPH and ABTS, and can inhibit the production of ROS in skin and intestinal cells within a certain concentration range. The higher the concentration of chitosan-nanoselenium, the greater the inhibition of ROS. In addition, nano-selenium can also exert an antioxidant effect by inhibiting cell apoptosis. Nano-selenium can regulate the permeability of mitochondrial membrane channels by upregulating the expression of anti-apoptotic protein Bcl-2 and downregulating the expression of apoptotic protein Bax, inhibiting the release of pro-apoptotic proteins into the cytoplasm, thereby inhibiting the occurrence of cell apoptosis.

[0004] At present, the preparation methods of nano-selenium are mainly divided into biosynthesis, physical synthesis and chemical synthesis. However, the shape, size and functional characteristics of nano-selenium prepared by biosynthesis depend on the selected strains, so it is difficult to control the morphology and size of the product. Although the physical synthesis method is simple to operate, the equipment cost is high and the generated nano-selenium is not stable and easy to aggregate. Nano-selenium prepared by chemical synthesis has a strong surface energy. In the absence of dispersants and stabilizers, selenium elements are prone to aggregation and precipitation, which affects the particle size, bioavailability and biological activity of nano-selenium. Summary of the invention

[0005] The purpose of the present invention is to solve the deficiencies of the prior art, add a psyllium polysaccharide template during the redox reaction to prevent the aggregation of nano-selenium particles, enhance their stability, and improve their biological activity. Provide a psyllium polysaccharide-nanoselenium complex and its preparation method and application, specifically using the following technical solutions: In one aspect of the present invention, a method for preparing plantago polysaccharide-nanoselenium is provided, comprising the following steps: S1: Soak the psyllium powder in 80% ethanol for 12 h-24 h, then filter and dry to obtain a filter residue; S2: placing the filter residue in water, reflux in a boiling water bath, centrifuge, filter, extract, and obtain a filtrate; S3: vacuum concentrating the filtrate, ethanol precipitation, centrifugation, and washing to obtain polysaccharide precipitate; S4: re-dissolving the polysaccharide precipitate, adding papain to hydrolyze and inactivate the enzyme, and then deproteinizing by Sevag method, dialyzing, and freeze-drying to obtain Plantago polysaccharide; S5: dissolving psyllium polysaccharide in water to obtain psyllium polysaccharide solution, adding sodium selenite solution to mix, then dropping ascorbic acid solution, reacting in a constant temperature water bath, dialyzing after the reaction, freeze-drying, and finally obtaining psyllium polysaccharide-nanoselenium.

[0006] Since the purity of polysaccharide will affect the particle size of the prepared nano-selenium, and the purity of psyllium polysaccharide purchased on the market is too high, the template component as a stable nano-selenium is relatively single, the present invention adopts water extraction and alcohol precipitation method to extract psyllium polysaccharide, psyllium polysaccharide is used as a dispersant and stabilizer, sodium selenite is used as an oxidant, and ascorbic acid is used as a reducing agent, and psyllium polysaccharide-nano-selenium is prepared by oxidation-reduction principle. Wherein psyllium polysaccharide is a biomacromolecule polysaccharide, which not only has the effects of anti-oxidation, hypoglycemic, hypolipidemic, immunomodulation, etc., but also has a complex branched structure and abundant hydroxyl groups. In the reaction system for preparing nano-selenium, the initially formed nano-selenium can be wrapped by physical adsorption to prevent the nano-particles from agglomerating and precipitating, and obtain nano-selenium particles with smaller particle size and higher stability. The content of selenium in the prepared psyllium polysaccharide-nano-selenium solution is 32 mg / L, accounting for 60.77% of the total amount of selenium in the original sodium selenite, as measured by inductively coupled plasma emission spectrometer. Transmission electron microscopy and scanning electron microscopy images showed that the psyllium polysaccharide-nanoselenium was a single, complete and uniform spherical particle tightly arranged and stacked. The ultraviolet scanning spectrum showed that the psyllium polysaccharide-nanoselenium had an obvious absorption peak at 268 nm, indicating that nanoselenium was generated. The infrared spectrum results showed that no new chemical bonds were generated during the preparation process, and the two were mainly physically combined through intermolecular forces such as hydrogen bonds and van der Waals forces. The X-ray photoelectron spectroscopy results showed that there was only zero-valent selenium in the psyllium polysaccharide-nanoselenium without highly toxic tetravalent selenium ions. The particle size and potential analysis showed that the particle size of the psyllium polysaccharide-nanoselenium was 78.39 nm, the dispersion coefficient PDI was 0.19, and the Zeta potential value was -33.7 mV.

[0007] As a further preferred embodiment, the mass ratio of psyllium powder to 80% ethanol is 1:8.

[0008] As a further preferred embodiment, the mass ratio of filter residue to water is 1:10.

[0009] As a further preferred embodiment, the concentration of the psyllium polysaccharide solution is 0.04 mg / mL. If the concentration of the psyllium polysaccharide solution is too high, the size of the prepared nano-selenium particles will be too large. If the concentration is too low, the nascent nano-selenium particles cannot be completely coated, making them easy to aggregate and precipitate. The concentration of the sodium selenite solution is 2 mM. The concentration of the ascorbic acid solution is 10 mM. If the concentration of the ascorbic acid solution is too high, it will not significantly reduce the particle size of the nano-selenium particles, but will cause unnecessary waste. If the concentration is too low, a large amount of toxic selenium ions will appear in the system due to the lack of sufficient reducing agent and the nano-selenium yield will be reduced.

[0010] As a further preferred embodiment, the volume ratio of the psyllium polysaccharide solution, the sodium selenite solution and the ascorbic acid solution is 1:1:1. If the volume ratio of the psyllium polysaccharide solution is too large, the nano-selenium particles will be over-coated and thus increase their particle size, while if the volume ratio of the reactants is too large, excessive nano-selenium particles will be generated and cannot be completely coated by the polysaccharide, thereby causing the particles to adsorb and precipitate each other.

[0011] As a further preferred embodiment, the enzymatic hydrolysis temperature is 60°C for 2 h, and the enzyme inactivation temperature is 95°C for 0.5 h, so as to fully remove the protein in the polysaccharide.

[0012] As a further preferred embodiment, the temperature of the constant temperature water bath reaction is 60°C and the reaction time is 1.5 h. Too high a temperature or too long a reaction time will significantly increase the particle size of the nano-selenium, while too low a temperature or too short a reaction time will result in insufficient combination of the plantago polysaccharide template and the nano-selenium.

[0013] The second aspect of the present invention provides a plantago polysaccharide-nano-selenium prepared by the above preparation method, wherein the plantago polysaccharide-nano-selenium has a selenium content of 32 mg / L.

[0014] The third aspect of the present invention also provides the use of the above-mentioned Plantago polysaccharide-nanoselenium in the preparation of antioxidant drugs or health products.

[0015] The beneficial effects of the present invention are: (1) The present invention adopts water extraction and alcohol precipitation method to extract psyllium polysaccharide, uses psyllium polysaccharide as dispersant and stabilizer, sodium selenite as oxidant, and ascorbic acid as reductant, and prepares psyllium polysaccharide-nanoselenium by oxidation-reduction principle. The results of in vitro antioxidant experiment of the psyllium polysaccharide-nanoselenium in the embodiment of the present invention show that the scavenging ability of psyllium polysaccharide-nanoselenium on DPPH free radical, hydroxyl free radical and ABTS free radical is concentration-dependent. When the concentration of psyllium polysaccharide-nanoselenium is 32 μg / mL, the scavenging ability of PLP-SeNPs on DPPH free radical, hydroxyl free radical and ABTS free radical is as high as 49.49 ± 2.58%, 60.99 ± 2.49% and 42.07 ± 1.76%, which is significantly higher than that of psyllium polysaccharide and nanoselenium, indicating that psyllium polysaccharide modification can significantly improve the antioxidant activity of nanoselenium; (2) The present invention prepares a psyllium polysaccharide-nanoselenium complex with small particle size, high electrostatic stability and higher antioxidant activity. The preparation method is simple and easy to operate, takes a short time, does not involve strong acid and alkali chemical reagents in the reaction system, is green and safe, has a high selenium content in the product and a stable system. The present invention provides a theoretical basis for the research and development of psyllium polysaccharide-nanoselenium and selenium-rich functional foods, and provides a theoretical basis for the development of new health foods and drugs. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The figure shows the actual image of the psyllium polysaccharide-nanoselenium prepared by the present invention; Figure 2 Shown are transmission electron microscope and scanning electron microscope images of psyllium polysaccharide-nano-selenium in the characterization experiment of psyllium polysaccharide-nano-selenium particles prepared by the present invention; Figure 3 The figure shows the ultraviolet spectrum of psyllium polysaccharide-nano-selenium in the characterization experiment of psyllium polysaccharide-nano-selenium particles prepared by the present invention; Figure 4 The figure shows the infrared spectrum of psyllium polysaccharide-nano-selenium in the characterization experiment of psyllium polysaccharide-nano-selenium particles prepared by the present invention; Figure 5 The figure shows the X-ray photoelectron spectrum of the psyllium polysaccharide-nano-selenium peaks after fitting in the characterization experiment of the psyllium polysaccharide-nano-selenium particles prepared by the present invention; Figure 6 Shown is a comparison chart of the scavenging rates of psyllium polysaccharide-nano-selenium on DPPH free radicals, hydroxyl free radicals and ABTS free radicals in an in vitro antioxidant experiment of psyllium polysaccharide-nano-selenium particles prepared by the present invention. DETAILED DESCRIPTION

[0017] The following will be combined with the embodiments and drawings to clearly and completely describe the concept, specific structure and technical effects of the present invention, so as to fully understand the purpose, scheme and effect of the present invention. It should be noted that the embodiments and features in the embodiments of this application can be combined with each other without conflict.

[0018] Example 1 A method for preparing plantago polysaccharide-nanoselenium, which specifically comprises the following steps: Step 1: The crushed psyllium powder that passed through an 80-mesh sieve was added to 80% ethanol at a solid-liquid ratio of 1:8 (mass ratio) and soaked for 24 hours. The filter residue was dried in the shade and added to ultrapure water at a solid-liquid ratio of 1:10 (mass ratio). The mixture was refluxed in a boiling water bath for 3 hours, centrifuged at 4800 r / min for 10 minutes and filtered with gauze. The filter residue was extracted twice, the filtrate was collected, vacuum concentrated, alcohol precipitated overnight, centrifuged at 4800 r / min for 10 minutes, the polysaccharide precipitate was collected and washed twice with acetone, ether, and anhydrous ethanol. The polysaccharide precipitate was redissolved, papain (1.5 g / L) was added, and the enzyme was hydrolyzed at 60℃ for 2 hours, the enzyme was inactivated at 95℃ for 0.5 hours, and the protein was repeatedly deproteinized by the Sevag method (chloroform: n-butanol = 4:1), dialyzed with running tap water for 48 hours, dialyzed with distilled water for 24 hours, and then freeze-dried to obtain psyllium polysaccharide; Step 2: Prepare 0.04 mg / mL psyllium polysaccharide solution, 2 mM sodium selenite solution and 10 mM ascorbic acid solution by mixing psyllium polysaccharide, sodium selenite, ascorbic acid and ultrapure water; Step 3: Take a 50 mL beaker and place it on a heat-collecting magnetic stirrer. Add 5 mL of psyllium polysaccharide solution and 5 mL of sodium selenite solution to the beaker, slowly drop 5 mL of ascorbic acid solution (molar ratio of reactants is 1:5), keep it in a constant temperature water bath at 60°C for 1.5 h, dialyze it with ultrapure water for 48 h, and replace the ultrapure water every 4 h to obtain psyllium polysaccharide-nanoselenium solution (such as Figure 1 As shown), the mixture was centrifuged at 12000 r / min for 30 min to obtain a nano-selenium solution, and the psyllium polysaccharide-nano-selenium solution was freeze-dried to obtain psyllium polysaccharide-nano-selenium.

[0019] The prepared Plantago polysaccharide-nanoselenium was characterized and analyzed (1) The psyllium polysaccharide-nanoselenium solution was subjected to particle size and potential analysis, inductively coupled plasma emission spectroscopy detection and ultraviolet full wavelength scanning; (2) The psyllium polysaccharide-nanoselenium sample was subjected to transmission electron microscopy, infrared spectroscopy scanning and X-ray photoelectron spectroscopy analysis; The results are as follows Figure 2-Figure 5 shown by Figure 2-Figure 5 It can be seen that the particle size of psyllium polysaccharide-nanoselenium is 78.39 ± 2.15 nm, the PDI value is 0.19 ± 0.10, the Zeta potential value is -(33.7 ± 0.76) mV, and the selenium content in psyllium polysaccharide-nanoselenium is (32 ± 2) mg / L, accounting for (60.77 ± 3.83)% of the total selenium in the original sodium selenite. Psyllium polysaccharide-nanoselenium with small particle size, high electrostatic stability and high yield was prepared. It can be seen from the transmission electron microscopy and scanning electron microscopy images that the nanoselenium modified by psyllium polysaccharide is a single complete and uniform spherical particle tightly arranged and stacked. Existing studies have shown that nanoselenium has a characteristic peak around 260 nm. The ultraviolet scanning spectrum of psyllium polysaccharide-nanoselenium shows that the sample has an obvious absorption peak at 268 nm, indicating that nanoselenium is generated. The results of Fourier infrared spectrometer showed that psyllium polysaccharide and psyllium polysaccharide-nanoselenium had highly similar absorption peaks in the fingerprint area, indicating that psyllium polysaccharide was combined with nanoselenium. No new absorption peak appeared, indicating that no new chemical bond was generated. The two were mainly physically combined through intermolecular forces such as hydrogen bonds and van der Waals forces. −1 The broad and strong peak at 2925.54 cm −1 The absorption peak at 1639.89 cm −1The absorption peak at 1430.46 cm −1 The absorption peak at 1048.55 cm-1 can be attributed to the asymmetric and symmetric stretching vibrations of the carboxylic acid group, indicating the presence of carboxyl groups in psyllium polysaccharide. −1 The absorption peak at belongs to the stretching vibration of the pyranoside ether bond COC. The characteristic absorption peaks of the above-mentioned psyllium polysaccharides all underwent blue shifts to varying degrees, indicating that -OH, -NH2, -C=O, COC, etc. of psyllium polysaccharides may be the main groups for binding to nano-selenium, indicating that the polysaccharide part containing a large amount of -OH, -C=O, and COC in psyllium polysaccharides may bind to nano-selenium and form a stable spherical structure. X-ray photoelectron spectroscopy analysis showed that the Se 3d5 / 2 electron binding energy peak position of 55.4 and the Se 3d3 / 2 electron binding energy peak position of 56.3 in the psyllium polysaccharide-nanoselenium sample were both zero-valent selenium electron binding energy peak positions, indicating that the selenium element in psyllium polysaccharide-nanoselenium was zero-valent, indicating that the solution system reacted completely and all sodium selenite was reduced to zero-valent selenium.

[0020] Example 2 A method for preparing plantago polysaccharide-nanoselenium, which specifically comprises the following steps: Step 1: The crushed psyllium powder that passed through an 80-mesh sieve was added to 80% ethanol at a solid-liquid ratio of 1:8 (mass ratio) and soaked for 24 hours. The filter residue was dried in the shade and added to ultrapure water at a solid-liquid ratio of 1:10 (mass ratio). The mixture was refluxed in a boiling water bath for 3 hours, centrifuged at 4800 r / min for 10 minutes and filtered with gauze. The filter residue was extracted twice, the filtrate was collected, vacuum concentrated, alcohol precipitated overnight, centrifuged at 4800 r / min for 10 minutes, the polysaccharide precipitate was collected and washed twice with acetone, ether, and anhydrous ethanol. The polysaccharide precipitate was redissolved, papain (1.5 g / L) was added, and the enzyme was hydrolyzed at 60℃ for 2 hours, the enzyme was inactivated at 95℃ for 0.5 hours, and the protein was repeatedly deproteinized by the Sevag method (chloroform: n-butanol = 4:1), dialyzed with running tap water for 48 hours, dialyzed with distilled water for 24 hours, and then freeze-dried to obtain psyllium polysaccharide; Step 2: Prepare 0.06 mg / mL psyllium polysaccharide solution, 2 mM sodium selenite solution and 8 mM ascorbic acid solution by mixing psyllium polysaccharide, sodium selenite, ascorbic acid and ultrapure water; Step 3: Take a 50 mL beaker and place it on a heat-collecting magnetic stirrer. Add 5 mL of psyllium polysaccharide solution and 5 mL of sodium selenite solution into the beaker. Slowly add 5 mL of ascorbic acid solution (the molar ratio of sodium selenite to ascorbic acid is 1:4). Keep it in a constant temperature water bath at 40°C for 0.5 h. Dialyze with ultrapure water for 48 h. Replace the ultrapure water every 4 h to obtain psyllium polysaccharide-nanoselenium solution.

[0021] The prepared plantago polysaccharide-nanoselenium solution was subjected to particle size and potential analysis. After testing, the particle size of psyllium polysaccharide-nano selenium was 94.00 ± 2.21 nm, the PDI value was 0.31 ± 0.17, and the Zeta potential value was -(30.1 ± 0.86) mV. This indicates that the psyllium polysaccharide-nano selenium prepared under these conditions has a larger particle size, and its dispersibility and stability are worse than those of the psyllium polysaccharide-nano selenium product in Example 1, that is, the psyllium polysaccharide concentration, the molar ratio of sodium selenite and ascorbic acid, the reaction temperature and the reaction time will affect the particle size of psyllium polysaccharide-nano selenium, and thus affect its biological activity.

[0022] Example 3 The antioxidative activity of the psyllium polysaccharide, nano-selenium and psyllium polysaccharide-nano-selenium prepared in Example 1 was tested. (1) The DPPH free radical scavenging ability was tested according to the following method: Take 0.1 mM DPPH·ethanol solution and 100 μL of different concentration gradients of psyllium polysaccharide, psyllium polysaccharide-nanoselenium and Vc (positive control) solutions and add them to a 96-well plate (the concentrations of psyllium polysaccharide are 0.4156, 0.8313, 1.6625, 3.325, 6.65, 13.3 μg / mL, and the concentrations of nanoselenium, psyllium polysaccharide-nanoselenium complex and Vc solution are 1, 2, 4, 8, 16, 32 μg / mL), mix well, let stand in a dark environment at room temperature for 30 minutes, and measure the absorbance at a wavelength of 517 nm with an ELISA reader, with anhydrous ethanol as the blank. The scavenging rate of DPPH free radicals is calculated according to the following formula.

[0023] Where: Ai is the absorbance value after the sample and DPPH are mixed; Aj is the absorbance value after the sample and anhydrous ethanol are mixed; Ac is the absorbance value after ultrapure water and DPPH are mixed.

[0024] (2) The hydroxyl radical scavenging ability was tested according to the following method: 1 mM ferrous sulfate solution, 1 mM salicylic acid·ethanol solution, different concentration gradients of psyllium polysaccharide, psyllium polysaccharide-nanoselenium and Vc (positive control) solution (the concentration of psyllium polysaccharide was 0.4156, 0.8313, 1.6625, 3.325, 6.65, 13.3 μg / mL, the concentration of nanoselenium, psyllium polysaccharide-nanoselenium complex and Vc solution was 1, 2, 4, 8, 16, 32 μg / mL), 1 mM H2O2 solution, 50 μL each, were added to a 96-well plate, mixed evenly, and allowed to stand at room temperature in the dark for 30 minutes, and the absorbance was measured at a wavelength of 510 nm using an ELISA reader. The scavenging rate of hydroxyl radicals was calculated according to the following formula.

[0025] Where: Ai is the absorbance value after the sample and reagents such as ferrous sulfate are mixed; Aj is the absorbance value after the sample and ultrapure water are mixed; Ac is the absorbance value after ultrapure water and reagents such as ferrous sulfate are mixed.

[0026] (3) The free radical scavenging ability of ABTS was tested according to the following method: 2 mL of 7.4 mM ABTS solution and 2 mL of 2.5 mM potassium persulfate were mixed and placed in the dark for 12 h to obtain ABTS•+ solution, which was diluted with anhydrous ethanol to an absorbance of 0.70 ± 0.01 at 734 nm. 100 μL of plantago polysaccharide, plantago polysaccharide-nanoselenium and Vc (positive control) solutions with different concentrations and 100 μL of ABTS•+ solution were added to a 96-well plate (the concentrations of plantago polysaccharide were 0.4156, 0.8313, 1.6625, 3.325, 6.65, and 13.3 μg / mL, and the concentrations of nanoselenium, plantago polysaccharide-nanoselenium complex and Vc solution were 1, 2, 4, 8, 16, and 32 μg / mL), and mixed evenly. After 6 min of reaction in the dark, the absorbance was measured at 734 nm using an ELISA reader. The ABTS free radical scavenging rate was calculated according to the following formula.

[0027] Where: A0 is the absorbance value of the blank group; Ai is the absorbance value of the sample group.

[0028] The test results are as follows Figure 6 As shown. Figure 6It can be seen that the scavenging ability of psyllium polysaccharide-nanoselenium on DPPH, hydroxyl radicals and ABTS free radicals is dose-dependent, and the scavenging ability of psyllium polysaccharide-nanoselenium on the three free radicals is higher than that of psyllium polysaccharide and nanoselenium. At 32 μg / mL, the scavenging ability of PLP-SeNPs on DPPH free radicals, hydroxyl free radicals and ABTS free radicals is as high as 49.49 ± 2.58%, 60.99 ± 2.49% and 42.07 ± 1.76%, which is much higher than the free radical scavenging ability of PLP and SeNPs at the same concentration, indicating that the PLP-SeNPs complex has stronger antioxidant capacity. The order of scavenging ability of psyllium polysaccharide-nanoselenium on the three free radicals is hydroxyl free radical>DPPH free radical>ABTS free radical.

[0029] Although the description of the present invention has been quite detailed and specifically describes several described embodiments, it is not intended to be limited to any of these details or embodiments or any particular embodiment, but should be regarded as providing a broad possible interpretation of these claims in view of the prior art by reference to the appended claims, thereby effectively covering the intended scope of the present invention. In addition, the above description of the present invention is based on the embodiments foreseeable by the inventor, and its purpose is to provide a useful description, and those non-substantial changes to the present invention that have not yet been foreseen may still represent equivalent changes to the present invention.

Claims

1. A method for preparing plantago polysaccharide-nanoselenium, characterized in that: The following steps are involved: S1: Soak the psyllium powder in 80% ethanol for 12 h-24 h, then filter and dry to obtain a filter residue; S2: placing the filter residue in water, reflux in a boiling water bath, centrifuge, filter, extract, and obtain a filtrate; S3: vacuum concentrating the filtrate, ethanol precipitation, centrifugation, and washing to obtain polysaccharide precipitate; S4: re-dissolving the polysaccharide precipitate, adding papain to hydrolyze and inactivate the enzyme, and then deproteinizing by Sevag method, dialyzing, and freeze-drying to obtain Plantago polysaccharide; S5: dissolving psyllium polysaccharide in water to obtain psyllium polysaccharide solution, adding sodium selenite solution to mix, then dropping ascorbic acid solution, reacting in a constant temperature water bath, dialyzing after the reaction, freeze-drying, and finally obtaining psyllium polysaccharide-nanoselenium.

2. The preparation method according to claim 1, characterized in that: The mass ratio of psyllium powder to 80% ethanol is 1:

8.

3. The preparation method according to claim 1, characterized in that: The mass ratio of filter residue to water is 1:

10.

4. The preparation method according to claim 1, characterized in that: The concentration of the psyllium polysaccharide solution was 0.04 mg / mL, the concentration of the sodium selenite solution was 2 mM, and the concentration of the ascorbic acid solution was 10 mM.

5. The preparation method according to claim 4, characterized in that: The volume ratio of the psyllium polysaccharide solution, the sodium selenite solution and the ascorbic acid solution is 1:1:

1.

6. The preparation method according to claim 1, characterized in that: The temperature for enzymatic hydrolysis was 60℃ for 2 h, and the temperature for enzyme inactivation was 95℃ for 0.5 h.

7. The preparation method according to claim 1, characterized in that: The temperature of the constant temperature water bath reaction was 60°C and the reaction time was 1.5 h.

8. A plantago polysaccharide-nanoselenium, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.

9. The plantago polysaccharide-nanoselenium according to claim 8, characterized in that: The selenium content in the plantago polysaccharide-nanoselenium is 32 mg / L.

10. Use of the plantago nano-selenium according to any one of claims 8 to 9 in the preparation of antioxidant drugs or health products.

Citation Information

Patent Citations

  • Roxburgh rose polysaccharide functionalized nanometer selenium compound, preparation method thereof and application of roxburgh rose polysaccharide functionalized nanometer selenium compound in blood glucose reducing drug

    CN109303922A

  • Sargassum fusiforme polysaccharide functionalized nano-selenium as well as preparation method and application thereof

    CN112370465A

  • Preparation method of auricularia polytricha polysaccharide nano-selenium compound

    CN115089605A