Novel direct-pressure-grade mannitol particles
Through the combination of highly dispersed micro-powder silica gel and composite hydroxyapatite, and using hydrophobic modification and coating technology, the fluidity and stability problems of mannitol raw powder in the direct powder compression method were solved, and a product with good fluidity and New direct compression grade mannitol granules with high storage stability and improved tablet hardness.
Patent Information
- Application Number
- CN202411223575.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-09-03
AI Technical Summary
Mannitol raw powder has poor fluidity in the direct powder compression method, resulting in uneven mixing and low hardness of the prepared tablets. Micronized silica gel is easy to agglomerate and absorb moisture, resulting in unstable quality of mannitol particles and poor storage stability.
A combination of highly dispersed micropowder silica gel and composite hydroxyapatite is used to prepare hydrophobic micropowder silica gel through hydrophobic modification and coating technology, and is mixed with raw mannitol powder to prepare new direct-pressure grade mannitol particles through spray granulation technology.
The fluidity and storage stability of mannitol particles are improved, the particle quality is stabilized, the tablet hardness is enhanced, the fluidity and storage stability of mannitol particles are ensured, and the hardness of the prepared tablets reaches 148-155N.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pharmaceutical excipients, and in particular to a novel direct-compression grade mannitol granule. Background Art
[0002] Mannitol is a sugar alcohol that is easily soluble in water. It is a white crystalline powder with a sweet taste similar to sucrose. Mannitol is a good diuretic in medicine, which can reduce intracranial pressure and intraocular pressure. It can also be used as a kidney medicine and dehydration medicine. Due to its low hygroscopicity and good thermal stability, it is also often used as an excipient in the powder direct tableting method.
[0003] The direct powder compression method refers to a method of directly compressing a mixture of drugs and excipients without going through a granulation process. The direct powder compression method avoids the granulation process and has the advantages of saving time and energy, simple process, and fewer steps. It is suitable for drugs that are unstable to moisture and heat. Commonly used excipients in the direct powder compression method include microcrystalline cellulose, anhydrous lactose, pregelatinized starch, povidone, etc. In addition, a flow aid is also required in the direct powder compression method to improve processing fluidity and compression molding. The commonly used flow aid is micro-powder silica gel. Micro-powder silica gel can fill the rough part of the powder surface to form a smooth surface, thereby reducing the friction and electrostatic force between particles, thereby reducing the adhesion, cohesion, and friction between particles, thereby improving the fluidity of the powder.
[0004] When mannitol is used as an excipient in a direct powder compression method, the original mannitol powder is a white needle-shaped crystal with poor fluidity. Considering the problem of uneven mixing between the drug and the excipients in the direct powder compression method itself, the original mannitol powder cannot be directly used in the direct powder compression method. In order to solve this problem, the commonly used method is to prepare mannitol granules from the original mannitol powder by spray drying or melt extrusion.
[0005] However, the tablet hardness of the tablets prepared from the above-mentioned mannitol granules is low. In order to solve this problem, the inventors tried to prepare mannitol granules with good fluidity and high tablet hardness by compounding micro-powder silica gel with mannitol raw powder. However, since the micro-powder silica gel is easy to agglomerate, the quality of the prepared mannitol granules will be unstable. Moreover, since the micro-powder silica gel is easy to absorb moisture, the storage stability of the prepared mannitol granules will also be poor. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a novel direct compression grade mannitol granules with good fluidity and storage stability and stable quality. The tablets prepared from the novel direct compression grade mannitol granules of the present invention have high tablet hardness.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: A novel direct compression grade mannitol granule is prepared by the following steps: preparing highly dispersed micro powder silica gel, preparing composite hydroxyapatite, mixing, and spray granulation; The method for preparing highly dispersed micro powder silica gel comprises the following steps: hydrophobic modification and coating; The hydrophobic modification comprises mixing micropowder silica gel and the first portion of anhydrous ethanol, and oscillating the mixture at an ultrasonic frequency of 20-25 kHz for 30-40 minutes at room temperature to obtain a micropowder silica gel dispersion; mixing stearic acid and the second portion of anhydrous ethanol, and stirring the mixture at 40-50° C. and 300-400 rpm for 10-15 minutes, adding the micropowder silica gel dispersion, and continuing to stir the mixture for 30-40 minutes after the addition is completed, filtering, washing the filter cake with anhydrous ethanol for 3-4 times, and then drying and crushing the filter cake to obtain hydrophobic micropowder silica gel; In the hydrophobic modification, the mass ratio of micropowder silica gel, the first portion of anhydrous ethanol, stearic acid, and the second portion of anhydrous ethanol is 100-110:1700-2000:20-25:3500-4000; The addition rate of the micropowder silica gel dispersion is 15-20 g / min; The average particle size of the micropowder silica gel is 10 μm; The coating comprises mixing the hydrophobic silica gel powder and the first portion of deionized water, and oscillating the mixture at an ultrasonic frequency of 20-25 kHz for 45-55 minutes at room temperature to obtain a hydrophobic silica gel powder dispersion; mixing the polyethylene glycol-polylactic acid block copolymer and the second portion of deionized water, and stirring the mixture at a stirring speed of 300-400 rpm for 20-30 minutes at room temperature, adding the hydrophobic silica gel powder dispersion, and continuing to stir the mixture for 30-40 minutes after the addition is completed, filtering, washing the filter cake with deionized water for 3-4 times, and then drying and crushing the filter cake to obtain a highly dispersed silica gel powder; In the coating, the mass ratio of hydrophobic micropowder silica gel, the first portion of deionized water, polyethylene glycol-polylactic acid block copolymer, and the second portion of deionized water is 110-115:2500-3000:200-230:4500-5000; The addition rate of the hydrophobic micropowder silica gel dispersion is 30-40 g / min; The weight average molecular weight of the polyethylene glycol-polylactic acid block copolymer is 10,000, the weight average molecular weight of the polyethylene glycol block is 4,000, and the weight average molecular weight of the polylactic acid block is 6,000; The composite hydroxyapatite is prepared by mixing alginic acid and the first portion of deionized water, stirring at 40-45° C. at a stirring speed of 400-500 rpm for 30-40 minutes, adding potassium dihydrogen phosphate, stirring for 20-30 minutes, adding anhydrous calcium chloride, stirring for 40-50 minutes, adding sodium hydroxide aqueous solution to adjust the pH to 10.5-11.5, continuing to stir for 3-3.5 hours after the addition is completed, standing at 40-45° C. for 14-15 hours, and centrifuging at a centrifugal speed of 5000-6000 rpm. 10-12min, take the precipitate, wash the precipitate with deionized water for 3-4 times, freeze-dry the precipitate, mix it with trehalose and the second portion of deionized water, stir it at a stirring speed of 400-500rpm for 5-6h at room temperature, centrifuge it at a centrifugal speed of 5000-6000rpm for 10-12min, take the precipitate, freeze-dry the precipitate, and ball-mill it, control the ball-to-material ratio during ball milling to be 4-5:1, the rotation speed to be 250-300rpm, and the time to be 50-60min, to obtain composite hydroxyapatite; In the preparation of the composite hydroxyapatite, the mass ratio of alginic acid, the first portion of deionized water, potassium dihydrogen phosphate, anhydrous calcium chloride, trehalose, and the second portion of deionized water is 45-50:2500-3000:250-260:340-355:65-70:2000-2200; The mass concentration of the sodium hydroxide aqueous solution is 10%; The addition rate of the sodium hydroxide aqueous solution is 6-7 g / min; The mixing comprises mixing highly dispersed micropowder silica gel, hydroxypropyl methylcellulose and the first portion of deionized water, stirring at a stirring speed of 200-300 rpm for 30-40 min at room temperature, adding composite hydroxyapatite, mannitol original powder and the second portion of deionized water, and continuing to stir for 1-1.5 h to obtain a mixed slurry; In the mixing, the mass ratio of highly dispersed micropowder silica gel, hydroxypropyl methylcellulose, the first portion of deionized water, composite hydroxyapatite, mannitol original powder, and the second portion of deionized water is 6-7:23-25:320-350:100-120:800-850:1500-1600; The average particle size of the mannitol raw powder is 50 μm; The spray granulation comprises adding the mixed slurry into a spray drying tower for spray drying, controlling the air inlet temperature to be 200-220° C. and the air outlet temperature to be 110-120° C., then passing through an 80-mesh sieve, taking the undersize, passing through a 150-mesh sieve, taking the oversize, and obtaining novel direct compression grade mannitol granules.
[0008] Compared with the prior art, the present invention has the following beneficial effects: (1) The novel direct compression grade mannitol granules of the present invention are prepared by adding highly dispersed micro-powder silica gel and composite hydroxyapatite, wherein the preparation method of the highly dispersed micro-powder silica gel comprises hydrophobic modification and coating, wherein the hydrophobic modification is to modify the surface of the micro-powder silica gel using hydrophobic stearic acid to obtain hydrophobic micro-powder silica gel, and the coating is to coat the hydrophobic micro-powder silica gel using a polyethylene glycol-polylactic acid block copolymer, and during the coating, the hydrophobic polylactic acid block faces the inside and the hydrophilic polyethylene glycol block faces the outside, thereby obtaining a highly dispersed micro-powder silica gel having a hydrophobic inner layer. The presence of the hydrophobic inner layer of the micro-powder silica gel reduces the moisture absorption of the new direct-compression grade mannitol particles and improves the storage stability of the new direct-compression grade mannitol particles; the hydrophobic modification and coating reduce the interaction between the micro-powder silica gels and improve the dispersibility of the micro-powder silica gel, thereby improving the fluidity of the new direct-compression grade mannitol particles and stabilizing the quality of the new direct-compression grade mannitol particles; the hydrophobic modification and coating can also improve the intermolecular interaction between the highly dispersed micro-powder silica gel and other components in the new direct-compression grade mannitol particles, thereby providing the preparation method. The preparation method of the composite hydroxyapatite is as follows: after mixing alginic acid with potassium dihydrogen phosphate and anhydrous calcium chloride, hydroxyapatite is generated in situ on the alginic acid to obtain a composite of alginic acid and hydroxyapatite, and then trehalose and the composite of alginic acid and hydroxyapatite are mixed, and trehalose is bound to the surface of the composite of alginic acid and hydroxyapatite through intermolecular forces, and then ball milling is performed to refine the composite of trehalose, alginic acid and hydroxyapatite, i.e., composite hydroxyapatite, and mannitol is added to the composite hydroxyapatite. During the mixing of the composite hydroxyapatite and the mannitol, mannitol is bound to the surface of the composite hydroxyapatite, thereby improving the fluidity of mannitol, further improving the fluidity of the new direct-compression grade mannitol granules, and stabilizing the quality of the new direct-compression grade mannitol granules; the new direct-compression grade mannitol granules are prepared by mixing the composite hydroxyapatite and mannitol, thereby reducing the hygroscopicity of trehalose and improving the storage stability of the new direct-compression grade mannitol granules; the presence of hydroxyapatite in the composite hydroxyapatite can also improve the tablet hardness of the tablets prepared from the new direct-compression grade mannitol granules; (2) The novel direct compression grade mannitol granules of the present invention have good fluidity, a bulk density of 497-529 g / L, and an angle of repose of 31-34°; (3) The novel direct compression grade mannitol granules of the present invention have good storage stability. When spread evenly in an environment with a temperature of 25°C and a relative humidity of 70%, there is no moisture problem after 5 days. (4) The novel direct compression grade mannitol granules of the present invention have stable quality. Three batches of samples were randomly selected, and the difference between the maximum bulk density and the minimum bulk density was 8-15 g / L, and the difference between the maximum angle of repose and the minimum angle of repose was 1-2°; (5) The tablets prepared from the novel direct compression grade mannitol granules of the present invention have high tablet hardness, which can reach 148-155N. DETAILED DESCRIPTION
[0009] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0010] Example 1 A novel direct compression grade mannitol granules is prepared by the following steps: 1. Preparation of highly dispersed micro powder silica gel: (1) Hydrophobic modification: 100 g of silica gel powder and 1700 g of anhydrous ethanol were mixed, and the mixture was oscillated at an ultrasonic frequency of 20 kHz for 30 min at room temperature to obtain a silica gel powder dispersion; 20 g of stearic acid and 3500 g of anhydrous ethanol were mixed, and the mixture was stirred at 300 rpm for 10 min at 40°C, and the above-mentioned silica gel powder dispersion was slowly added at a rate of 15 g / min. After the addition was completed, stirring was continued for 30 min, and the mixture was filtered. The filter cake was washed three times with anhydrous ethanol, and then the filter cake was dried and crushed to obtain hydrophobic silica gel powder; The average particle size of the micropowder silica gel is 10 μm; (2) Coating: 110 g of hydrophobic silica powder and 2500 g of deionized water were mixed, and the mixture was oscillated at an ultrasonic frequency of 20 kHz for 45 min at room temperature to obtain a hydrophobic silica powder dispersion; 200 g of polyethylene glycol-polylactic acid block copolymer and 4500 g of deionized water were mixed, and the mixture was stirred at a stirring speed of 300 rpm for 20 min at room temperature, and the above hydrophobic silica powder dispersion was slowly added at a rate of 30 g / min. After the addition was completed, stirring was continued for 30 min, and the mixture was filtered. After the filter cake was washed three times with deionized water, the filter cake was dried and crushed to obtain a highly dispersed silica powder; The weight average molecular weight of the polyethylene glycol-polylactic acid block copolymer is 10,000, the weight average molecular weight of the polyethylene glycol block is 4,000, and the weight average molecular weight of the polylactic acid block is 6,000; 2. Preparation of composite hydroxyapatite: 45g of alginic acid and 2500g of deionized water were mixed, stirred at 40°C at a stirring speed of 400rpm for 30min, 250g of potassium dihydrogen phosphate was added, stirred for 20-30min, 340g of anhydrous calcium chloride was added, stirred for 40min, and 10% sodium hydroxide aqueous solution was slowly added to adjust the pH to 10.5, and the addition speed was controlled to 6g / min. After the addition was completed, stirring was continued for 3h, and it was allowed to stand at 40°C for 14h. The mixture was centrifuged at a centrifugal speed of 5000 rpm for 10 min, and a precipitate was taken. The precipitate was washed with deionized water for 3 times, and then freeze-dried. The mixture was mixed with 65 g of trehalose and 2000 g of deionized water, and then stirred at a stirring speed of 400 rpm for 5 h at room temperature. The mixture was centrifuged at a centrifugal speed of 5000 rpm for 10 min, and a precipitate was taken. The precipitate was freeze-dried and then ball-milled. The ball-to-material ratio during ball milling was controlled to be 4:1, the rotation speed was 250 rpm, and the time was 50 min to obtain composite hydroxyapatite. 3. Mixing: After mixing the highly dispersed micro powder silica gel, hydroxypropyl methylcellulose and the first portion of deionized water, stir at room temperature at a stirring speed of 200 rpm for 30 minutes, add the composite hydroxyapatite, mannitol original powder and the second portion of deionized water, and continue stirring for 1 hour to obtain a mixed slurry; The mass ratio of highly dispersed micro powder silica gel, hydroxypropyl methylcellulose, the first portion of deionized water, composite hydroxyapatite, mannitol original powder, and the second portion of deionized water is 6:23:320:100:800:1500; The average particle size of the mannitol raw powder is 50 μm; 4. Spray granulation: Add the mixed slurry into a spray drying tower for spray drying, control the inlet air temperature to 200°C and the outlet air temperature to 110°C, then pass through an 80-mesh sieve, take the undersize, pass through a 150-mesh sieve, take the oversize, and obtain new direct compression grade mannitol granules.
[0011] Example 2 A novel direct compression grade mannitol granules is prepared by the following steps: 1. Preparation of highly dispersed micro powder silica gel: (1) Hydrophobic modification: 105 g of micro-powder silica gel and 1800 g of anhydrous ethanol were mixed, and the mixture was oscillated at an ultrasonic frequency of 20 kHz for 35 min at room temperature to obtain a micro-powder silica gel dispersion; 22 g of stearic acid and 3800 g of anhydrous ethanol were mixed, and the mixture was stirred at 350 rpm for 12 min at 45 °C, and the entire micro-powder silica gel dispersion was slowly added at a rate of 18 g / min. After the addition was completed, the mixture was stirred for 35 min, and the mixture was filtered. The filter cake was washed three times with anhydrous ethanol, and then dried and crushed to obtain hydrophobic micro-powder silica gel; The average particle size of the micropowder silica gel is 10 μm; (2) Coating: 112 g of hydrophobic silica powder and 2800 g of deionized water were mixed, and the mixture was oscillated at an ultrasonic frequency of 20 kHz for 50 min at room temperature to obtain a hydrophobic silica powder dispersion; 220 g of polyethylene glycol-polylactic acid block copolymer and 4800 g of deionized water were mixed, and the mixture was stirred at a stirring speed of 350 rpm for 25 min at room temperature, and the above hydrophobic silica powder dispersion was slowly added at a rate of 35 g / min. After the addition was completed, the mixture was stirred for 35 min, and the mixture was filtered. The filter cake was washed with deionized water for 3 times, and then the filter cake was dried and crushed to obtain a highly dispersed silica powder; The weight average molecular weight of the polyethylene glycol-polylactic acid block copolymer is 10,000, the weight average molecular weight of the polyethylene glycol block is 4,000, and the weight average molecular weight of the polylactic acid block is 6,000; 2. Preparation of composite hydroxyapatite: 48g of alginic acid and 2800g of deionized water were mixed, stirred at 40°C at a stirring speed of 450rpm for 35min, 255g of potassium dihydrogen phosphate was added, stirred for 25min, 350g of anhydrous calcium chloride was added, stirred for 45min, and a 10% sodium hydroxide aqueous solution was slowly added to adjust the pH to 11, and the addition rate was controlled to 6g / min. After the addition was completed, stirring was continued for 3h, and the mixture was allowed to stand at 40°C for 14.5h, and then stirred at 550rpm for 2h. 0rpm for 11min, take the precipitate, wash the precipitate with deionized water for 3 times, freeze-dry the precipitate, mix it with 68g trehalose and 2100g deionized water, stir it at 450rpm for 5.5h at room temperature, centrifuge it at 5500rpm for 11min, take the precipitate, freeze-dry the precipitate, and then ball-mill with the ball-to-material ratio of 4:1, the rotation speed of 280rpm, and the time of 55min to obtain composite hydroxyapatite; 3. Mixing: After mixing the highly dispersed micro-powder silica gel, hydroxypropyl methylcellulose and the first portion of deionized water, stir at room temperature at a stirring speed of 250 rpm for 35 minutes, add the composite hydroxyapatite, mannitol original powder and the second portion of deionized water, and continue stirring for 1 hour to obtain a mixed slurry; The mass ratio of highly dispersed micro powder silica gel, hydroxypropyl methylcellulose, the first portion of deionized water, composite hydroxyapatite, mannitol original powder, and the second portion of deionized water is 6:24:340:110:820:1550; The average particle size of the mannitol raw powder is 50 μm; 4. Spray granulation: Add the mixed slurry into a spray drying tower for spray drying, control the inlet air temperature to 210°C and the outlet air temperature to 115°C, then pass through an 80-mesh sieve, take the undersize, pass through a 150-mesh sieve, take the oversize, and obtain new direct compression grade mannitol granules.
[0012] Example 3 A novel direct compression grade mannitol granules is prepared by the following steps: 1. Preparation of highly dispersed micro powder silica gel: (1) Hydrophobic modification: 110 g of silica gel powder and 2000 g of anhydrous ethanol were mixed, and the mixture was oscillated at an ultrasonic frequency of 25 kHz for 40 min at room temperature to obtain a silica gel powder dispersion; 25 g of stearic acid and 4000 g of anhydrous ethanol were mixed, and the mixture was stirred at 400 rpm for 15 min at 50 °C, and the above-mentioned silica gel powder dispersion was slowly added at a rate of 20 g / min. After the addition was completed, stirring was continued for 40 min, and the mixture was filtered. After the filter cake was washed four times with anhydrous ethanol, the filter cake was dried and crushed to obtain hydrophobic silica gel powder; The average particle size of the micropowder silica gel is 10 μm; (2) Coating: 115 g of hydrophobic silica powder and 3000 g of deionized water were mixed, and the mixture was ultrasonically oscillated at 25 kHz for 55 min at room temperature to obtain a hydrophobic silica powder dispersion. 230 g of polyethylene glycol-polylactic acid block copolymer and 5000 g of deionized water were mixed, and the mixture was stirred at 400 rpm for 30 min at room temperature. The hydrophobic silica powder dispersion was slowly added at a rate of 40 g / min. After the addition was completed, the mixture was stirred for 40 min. The mixture was filtered, and the filter cake was washed with deionized water for 4 times. The filter cake was dried and crushed to obtain a highly dispersed silica powder. The weight average molecular weight of the polyethylene glycol-polylactic acid block copolymer is 10,000, the weight average molecular weight of the polyethylene glycol block is 4,000, and the weight average molecular weight of the polylactic acid block is 6,000; 2. Preparation of composite hydroxyapatite: 50g of alginic acid and 3000g of deionized water were mixed, stirred at 45°C at a stirring speed of 500rpm for 40min, 260g of potassium dihydrogen phosphate was added, stirred for 30min, 355g of anhydrous calcium chloride was added, stirred for 50min, and 10% sodium hydroxide aqueous solution was slowly added to adjust the pH to 11.5, and the addition rate was controlled to 7g / min. After the addition was completed, stirring was continued for 3.5h, and it was allowed to stand at 45°C for 15h. 000rpm for 12min, take the precipitate, wash the precipitate with deionized water for 4 times, freeze-dry the precipitate, mix it with 70g trehalose and 2200g deionized water, stir it at 500rpm for 6h at room temperature, centrifuge it at 6000rpm for 12min, take the precipitate, freeze-dry the precipitate, and then ball-mill with the ball-to-material ratio of 5:1, the rotation speed of 300rpm, and the time of 60min to obtain composite hydroxyapatite; 3. Mixing: After mixing the highly dispersed micro powder silica gel, hydroxypropyl methylcellulose and the first portion of deionized water, stir at room temperature at a stirring speed of 300 rpm for 40 minutes, add the composite hydroxyapatite, mannitol original powder and the second portion of deionized water, and continue stirring for 1.5 hours to obtain a mixed slurry; The mass ratio of highly dispersed micro powder silica gel, hydroxypropyl methylcellulose, the first portion of deionized water, composite hydroxyapatite, mannitol original powder, and the second portion of deionized water is 7:25:350:120:850:1600; The average particle size of the mannitol raw powder is 50 μm; 4. Spray granulation: Add the mixed slurry into a spray drying tower for spray drying, control the inlet air temperature to 220°C, the outlet air temperature to 120°C, then pass through an 80-mesh sieve, take the undersize, pass through a 150-mesh sieve, take the oversize, and obtain new direct compression grade mannitol granules.
[0013] Comparative Example 1 On the basis of the technical solution of Example 2, the step of preparing highly dispersed micro powder silica gel in step 1 is omitted, and in the mixing step in step 3, micro powder silica gel with an average particle size of 10 μm is used to replace the highly dispersed micro powder silica gel in an equal amount.
[0014] Comparative Example 2 On the basis of the technical solution of Example 2, the second step of preparing composite hydroxyapatite is omitted, and trehalose is used instead of composite hydroxyapatite in the third mixing step, and the mass ratio of trehalose to mannitol original powder is controlled to 15.6:800.
[0015] Test Example 1 According to the preparation steps of the novel direct-compression grade mannitol granules of Examples 1-3 and Comparative Examples 1-2, novel direct-compression grade mannitol granules were prepared respectively, and then three batches of samples were randomly selected from the prepared novel direct-compression grade mannitol granules, and the bulk density and repose angle were tested using Dandong BT-1001 intelligent powder property tester. The test results are as follows:
[0016] Test Example 2 According to the preparation steps of the novel direct-compression grade mannitol granules of Examples 1-3 and Comparative Examples 1-2, novel direct-compression grade mannitol granules were prepared respectively, and then 200 g of the novel direct-compression grade mannitol granules were taken respectively and spread in an environment with a temperature of 25° C. and a relative humidity of 70%. After 5 days, whether there was a moisture problem was observed, and the observation results were as follows:
[0017] Test Example 3 The novel direct compression grade mannitol granules of Examples 1-3 and Comparative Examples 1-2 were subjected to tableting performance tests, and the test methods and test methods were as follows: The novel direct compression grade mannitol granules of Examples 1-3 and Comparative Examples 1-2 were respectively mixed with magnesium stearate to control the mass content of magnesium stearate to be 1%, and then added to a ZPS-8 rotary tablet press, and tableted at a tableting pressure of 6 kN to obtain tablets with a diameter of 12 mm. 20 tablets were prepared from each novel direct compression grade mannitol granule, and the tablet hardness of each tablet was tested using a YPD-350N intelligent tablet hardness tester, and the average value was calculated. The calculation results are as follows:
[0018] It can be seen from the results of Experimental Examples 1-3 that by adding highly dispersed micropowder silica gel and composite hydroxyapatite in the preparation of the new direct compression grade mannitol granules, the fluidity and storage stability of the new direct compression grade mannitol granules can be improved, the quality of the new direct compression grade mannitol granules can be stabilized, and the tablet hardness of the prepared tablets can be improved.
[0019] Unless otherwise specified, all percentages used in the present invention are by mass.
[0020] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A novel direct compression grade mannitol granules, characterized in that: The method is prepared by the following steps: preparing highly dispersed micro powder silica gel, preparing composite hydroxyapatite, mixing, and spray granulating; The method for preparing highly dispersed micro powder silica gel comprises the following steps: hydrophobic modification and coating; The hydrophobic modification comprises mixing the micro-powder silica gel and the first portion of anhydrous ethanol evenly to obtain a micro-powder silica gel dispersion; mixing stearic acid and the second portion of anhydrous ethanol, stirring at 40-50° C., adding the micro-powder silica gel dispersion, continuing to stir after the addition is completed, filtering, washing, drying and crushing the filter cake to obtain hydrophobic micro-powder silica gel; The coating comprises mixing the hydrophobic silica gel powder and the first portion of deionized water evenly to obtain a hydrophobic silica gel powder dispersion; mixing the polyethylene glycol-polylactic acid block copolymer and the second portion of deionized water, stirring at room temperature, adding the hydrophobic silica gel powder dispersion, and continuing to stir after the addition is completed, filtering, washing, drying and crushing the filter cake to obtain a highly dispersed silica gel powder; The method for preparing the composite hydroxyapatite comprises mixing alginic acid and a first portion of deionized water, stirring at 40-45° C., adding potassium dihydrogen phosphate, stirring for 20-30 minutes, adding anhydrous calcium chloride, stirring, adding sodium hydroxide aqueous solution to adjust the pH to 10.5-11.5, continuing stirring after the addition, standing at 40-45° C., centrifuging, taking a precipitate, washing, freeze-drying the precipitate, mixing with trehalose and a second portion of deionized water, stirring at room temperature, centrifuging, taking a precipitate, freeze-drying the precipitate, and ball milling to obtain the composite hydroxyapatite; In the mixing, highly dispersed micro powder silica gel, hydroxypropyl methylcellulose and the first portion of deionized water are mixed, stirred at room temperature, composite hydroxyapatite, mannitol original powder and the second portion of deionized water are added, and stirring is continued to obtain a mixed slurry.
2. The novel direct compression grade mannitol granules according to claim 1, characterized in that: In the hydrophobic modification, the mass ratio of micropowder silica gel, the first portion of anhydrous ethanol, stearic acid, and the second portion of anhydrous ethanol is 100-110:1700-2000:20-25:3500-4000; The addition rate of the micropowder silica gel dispersion is 15-20 g / min; The average particle size of the micropowder silica gel is 10 μm.
3. The novel direct compression grade mannitol granules according to claim 1, characterized in that: In the coating, the mass ratio of hydrophobic micropowder silica gel, the first portion of deionized water, polyethylene glycol-polylactic acid block copolymer, and the second portion of deionized water is 110-115:2500-3000:200-230:4500-5000; The addition rate of the hydrophobic micropowder silica gel dispersion is 30-40 g / min; The weight average molecular weight of the polyethylene glycol-polylactic acid block copolymer is 10,000, the weight average molecular weight of the polyethylene glycol block is 4,000, and the weight average molecular weight of the polylactic acid block is 6,000.
4. The novel direct compression grade mannitol granules according to claim 1, characterized in that: In the preparation of the composite hydroxyapatite, the mass ratio of alginic acid, the first portion of deionized water, potassium dihydrogen phosphate, anhydrous calcium chloride, trehalose, and the second portion of deionized water is 45-50:2500-3000:250-260:340-355:65-70:2000-2200; The mass concentration of the sodium hydroxide aqueous solution is 10%; The addition rate of the sodium hydroxide aqueous solution is 6-7 g / min.
5. The novel direct compression grade mannitol granules according to claim 1, characterized in that: In the mixing, the mass ratio of highly dispersed micropowder silica gel, hydroxypropyl methylcellulose, the first portion of deionized water, composite hydroxyapatite, mannitol original powder, and the second portion of deionized water is 6-7:23-25:320-350:100-120:800-850:1500-1600; The average particle size of the mannitol raw powder is 50 μm.
6. The novel direct compression grade mannitol granules according to claim 1, characterized in that: The spray granulation comprises adding the mixed slurry into a spray drying tower for spray drying, then passing through an 80-mesh sieve, taking the undersize, passing through a 150-mesh sieve, taking the oversize, and obtaining novel direct compression grade mannitol granules; In the spray granulation, the inlet air temperature of the spray drying is 200-220°C, and the outlet air temperature is 110-120°C.
Citation Information
Patent Citations
Method for improving Chinese medicinal granula dry-method granulation formability and granula quality
CN108619099A
Direct-pressure-grade mannitol granules and preparation method thereof
CN117860688A
Fast-disintegrating compression molding and producing method thereof
JP2015078182A
Coated particle and method for producing coated particle
US20130071481A1