Polyimide hollow fiber membrane with polyion liquid side chain structure as well as preparation method and application of polyimide hollow fiber membrane
By constructing a polyionic liquid side chain structure on an aromatic polyimide hollow fiber membrane, the problem of insufficient heat resistance of existing membranes in high-temperature flue gas treatment is solved, high permeability and high selectivity are achieved, and it is suitable for The rapid transportation and separation of CO2 reduces production costs.
Patent Information
- Application Number
- CN202410971476.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing polyionic liquid membranes have insufficient heat resistance and mechanical properties in high-temperature flue gas treatment, and the cost is high, making it difficult to apply on a large scale. Moreover, the separation performance of ionic liquid-polymer blend membranes decreases at high temperatures, making it difficult to combine high Permeability and high selectivity.
Polyimide hollow fiber membranes with polyionic liquid side chain structures are used to build polyionic liquid segments on the aromatic polyimide main chain through atom transfer radical polymerization (ATRP) reaction to form a microphase separation structure and improve CO2 permeability and selectivity, and avoid ionic liquid overflow through chemical bonding.
It achieves high permeability, high selectivity and good heat resistance and mechanical properties. It is suitable for gas separation at high temperature and high pressure, reduces production costs, and is suitable for rapid transportation and separation of CO2.
Smart Images

Figure BDA0004953352860000031 
Figure BDA0004953352860000032 
Figure BDA0004953352860000061
Abstract
Description
Technical Field
[0001] The invention belongs to the field of gas separation membrane preparation, and particularly relates to a polyimide hollow fiber membrane with a polyionic liquid side chain structure, and a preparation method and application thereof. Background Art
[0002] As climate warming intensifies, extreme weather events around the world are becoming more frequent. People are urgently seeking green technology innovation to achieve clean production, reduce greenhouse gas emissions, and alleviate global warming. Membrane separation technology has the characteristics of energy saving and high efficiency, no secondary pollution, simple operation, and low cost, as it does not undergo phase change and does not require the addition of separation agents during the separation process. It is gradually becoming a research hotspot for CO2 separation.
[0003] Ionic liquids, also known as room temperature ionic liquids, room temperature molten salts or organic ionic liquids, are salts composed of organic cations and inorganic or organic anions that are in liquid state at room temperature or near room temperature. Due to the Lewis acid / base complexation between ionic liquids and CO2, they have a high solubility in CO2 and have been widely used in recent years to capture CO2 in industrial exhaust gas and natural gas. At present, gas separation membranes based on ionic liquids can be divided into polyionic liquid membranes and ionic liquid-polymer blend membranes. Polyionic liquid membranes are generally obtained by chemical polymerization of vinyl ionic liquid monomers. Since polyionic liquids are mostly alkane main chains, they have poor heat resistance and low thermal deformation temperature, making them difficult to use in actual scenarios such as high-temperature flue gas. In addition, this type of film is expensive and not convenient for large-scale application. Ionic liquid-polymer blend membranes refer to a certain amount of ionic liquid added to a polymer matrix material to improve the selectivity of the film for CO2. However, ionic liquids have a plasticizing effect on materials, which will reduce the heat resistance and mechanical properties of the separation membrane. When the ionic liquid content is too high, it is easy to agglomerate in the polymer matrix, hindering the transmission of CO2.
[0004] Aromatic polyimide is one of the most promising gas separation membrane materials because it contains a large number of rigid benzene ring structures, generally has a high free volume fraction, excellent thermal stability and chemical stability. However, the current aromatic polyimide gas separation membranes still have difficulty in achieving both high permeability and high selectivity.
[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a polyimide hollow fiber membrane having a polyionic liquid side chain structure.
[0006] The polyimide hollow fiber membrane with a polyionic liquid side chain structure obtained by the invention has excellent high permeability, high selectivity and mechanical properties.
[0007] Another object of the present invention is to provide a method for preparing the polyimide hollow fiber membrane having a polyionic liquid side chain structure.
[0008] Another object of the present invention is to provide application of the above-mentioned polyimide hollow fiber membrane having a polyionic liquid side chain structure in gas separation.
[0009] The purpose of the present invention is achieved through the following solutions:
[0010] A polyimide hollow fiber membrane with a polyionic liquid side chain structure comprises a polyimide main chain containing an alkyl group and a vinyl polyionic liquid side chain.
[0011] The method for preparing the above-mentioned polyimide hollow fiber membrane having a polyionic liquid side chain structure comprises the following steps:
[0012] (1) Under the protection of an inert atmosphere, a polyimide resin containing an alkyl structure, N-bromosuccinimide, and azobisisobutyronitrile are dissolved in an organic solvent, heated and stirred for reaction, and after the reaction is completed, the solution is poured into methanol for precipitation, and the obtained solid is a brominated polyimide resin;
[0013] (2) Under the protection of an inert atmosphere, a brominated polyimide resin, a vinyl ionic liquid monomer, a catalyst, and a ligand are dissolved in an organic solvent, heated and stirred to react, and after the reaction is completed, the solution is poured into methanol for precipitation, and the resulting solid is a polyimide resin having a polyionic liquid side chain structure;
[0014] (3) The polyimide resin having a polyionic liquid side chain structure is dissolved in an organic solvent, and the hollow fiber membrane is obtained by filtering, spinning, soaking and drying.
[0015] The number average molecular weight of the polyimide resin containing an alkyl structure in step (1) is 1,000 to 500,000.
[0016] The organic solvent in step (1) is one or more of chloroform, o-cresol, m-cresol, p-cresol, dimethyl sulfoxide, N-methylpyrrolidone, N,N-dimethylformamide and N,N-dimethylacetamide.
[0017] In step (1), the mass ratio of the polyimide resin containing an alkyl structure, N-bromosuccinimide and azobisisobutyronitrile is 100:(0.2-50):(0.001-0.5); the amount ratio of the polyimide resin containing an alkyl structure to the organic solvent is 1 g:(1-50) mL.
[0018] The reaction temperature of step (1) is 30-70°C and the reaction time is 12-48h.
[0019] The vinyl ionic liquid monomer in step (2) is at least one of the following compounds:
[0020]
[0021] Wherein, X is Cl, Br, I, COO, SCN, NO3, BF4 or PF6.
[0022] The catalyst in step (2) is a transition metal halide; preferably one of CuCl, CuBr and CuI.
[0023] The ligand in step (2) is one of the following compounds:
[0024]
[0025] The organic solvent in step (2) is one or more of dimethyl sulfoxide, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0026] In step (2), the mass ratio of the brominated polyimide resin, the vinyl ionic liquid monomer, the catalyst and the ligand is 100:(1-100):(0.01-0.5):(0.02-1); the amount ratio of the brominated polyimide resin to the organic solvent is 100g:(100-5000)mL.
[0027] The reaction temperature in step (2) is 60 to 120° C. and the reaction time is 12 to 36 hours.
[0028] The number average molecular weight of the polyimide resin having a polyionic liquid side chain structure obtained in step (2) is 5,000 to 1,000,000.
[0029] The organic solvent in step (3) is one or more of tetrahydrofuran, dimethyl sulfoxide, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0030] The amount of the organic solvent used in step (3) is such that the concentration of the polyimide resin having a polyionic liquid side chain structure in the spinning solution is 10 to 45 wt.%.
[0031] The mesh size of the filtration in step (3) is 300 to 500.
[0032] The spinning liquid in step (3) is the polyimide resin solution obtained after filtration, with a flow rate of 1 to 15 mL / min; the core liquid is a mixed solution of water and an organic solvent, with a flow rate of 0.2 to 5 mL / min, wherein the mass ratio of water to organic solvent is 50:50 to 10:90.
[0033] The coagulation bath for spinning in step (3) is water.
[0034] The immersion in step (3) is carried out by sequentially immersing in a methanol solution and n-hexane; wherein the immersion time is 1 to 5 hours, and the methanol concentration in the methanol solution is 70 to 90 wt.%.
[0035] The hollow fiber membrane in step (3) has an outer diameter of 200 to 500 μm, an inner diameter of 150 to 350 μm, and a membrane thickness of 40 to 100 μm.
[0036] The drying in step (3) is vacuum drying, the drying temperature is 100 to 150° C., and the drying time is 12 to 48 hours.
[0037] Application of the above-mentioned polyimide hollow fiber membrane with polyionic liquid side chain structure in gas separation.
[0038] The gas separation is to capture carbon dioxide from air, industrial flue gas, natural gas or biogas.
[0039] The mechanism of the present invention is:
[0040] The present invention provides a polyimide hollow fiber membrane with a polyionic liquid side chain structure and a preparation method thereof. The method utilizes an atom transfer radical polymerization (ATRP) reaction to fix a polyionic liquid fragment on an aromatic polyimide main chain. The active H on the imidazole ring in the polyionic liquid has a strong interaction with polar gases such as CO2, which can achieve highly selective and rapid transport of CO2 and improve the permeability of the membrane to polar gases such as CO2.
[0041] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0042] 1. The present invention utilizes ATRP reaction to construct polyionic liquid side chains on the main chain of aromatic polyimide. The active H on the polyionic liquid has a strong interaction with polar gases such as CO2, which can effectively enhance the material's solubility in polar gases such as CO2 and achieve highly selective and rapid transport of CO2.
[0043] 2. The compatibility structures of the aromatic polyimide main chain and the polyionic liquid side chain in the present invention are quite different. By preparing polyionic liquid side chains of appropriate length, a microphase separation structure can be formed in the film to construct a fast channel for gas molecule penetration.
[0044] 3. In the present invention, the polyionic liquid fragments are connected to the aromatic polyimide main chain through chemical bonds, which effectively avoids the phenomenon of ionic liquid overflowing due to high working pressure.
[0045] 4. The present invention adopts aromatic polyimide as the matrix material, and the obtained hollow fiber membrane has good heat resistance and mechanical properties, and can treat flue gas at a higher temperature and a higher pressure, thereby improving production efficiency.
[0046] 5. The present invention has universality. The method is applicable to all aromatic polyimide resins containing alkyl groups in their structures, and there is no need to prepare special diamine or dianhydride monomers with high preparation costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 The infrared spectra of the resins obtained in the comparative examples and embodiments are shown in FIG.
[0048] Figure 2 The separation performance of the hollow fiber membranes obtained in the comparative examples and examples for the CO2 / N2 gas pair.
[0049] Figure 3 The separation performance of the hollow fiber membranes obtained in the comparative examples and examples for the CO2 / CH4 gas pair.
[0050] Figure 4 The thermogravimetric curves of the hollow fiber membranes obtained in the comparative example and the example are shown.
[0051] Figure 5 It is a graph showing the mechanical tensile properties of the hollow fiber membranes obtained in the comparative example and the example. DETAILED DESCRIPTION
[0052] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0053] Unless otherwise specified, the reagents used in the examples can be purchased from the market.
[0054] Polyimide resin (PI):
[0055]
[0056] a) In a 250 mL three-necked flask, 50 mL of m-cresol solvent, 25 mL of toluene, 4.4424 g (0.01 mol) of hexafluorodianhydride (6FDA), 1.5023 g (0.01 mol) of 2,4,6-trimethyl-1,3-phenylenediamine and 0.1 g of isoquinoline were added in sequence, and after reflux and dehydration at 120 ° C for 6 h, the temperature was raised to 180 ° C for condensation for 12 h to obtain a polyimide solution. The condensation process was always carried out in a nitrogen atmosphere.
[0057] b) The polyimide solution is cooled to 80° C. and then slowly poured into anhydrous ethanol to precipitate white fibrous polyimide, which is washed by multiple exchanges with ethanol and then dried to obtain a polyimide resin (PI) material.
[0058] 1-vinyl-3-methylimidazolium iodide:
[0059] Where X is I;
[0060] Compound 1:
[0061]
[0062] Example 1
[0063] (1) Under nitrogen protection, add 150 mL of chloroform and 5.0 g of polyimide resin (PI) to a 250 mL three-necked flask, stir evenly, add 0.65 g of N-bromosuccinimide (NBS) and 0.004 g of azobisisobutyronitrile (AIBN), and heat to 60 °C for 24 h. After the reaction is completed, wait for the system to cool to room temperature and pour it into methanol for precipitation. Filter the precipitate, wash it several times, and then dry it to obtain PI-Br resin.
[0064] (2) Under nitrogen protection, add 150 mL of N-methylpyrrolidone (NMP) and 5.0 g of PI-Br resin to a 250 mL three-necked flask, stir evenly, add 0.5 g of 1-vinyl-3-methylimidazolium iodide, 0.02 g of CuCl and 0.03 g of compound 1, and heat to 70 ° C for 20 h. After the reaction is completed, wait for the system to cool to room temperature and pour it into methanol for precipitation. Filter the precipitate, wash it several times, and then dry it to obtain PI-PIL (10:1) resin.
[0065] (3) The dried PI-PIL (10:1) resin and NMP were mixed evenly at room temperature to obtain a spinning solution with a polymer content of 30 wt.%, which was filtered through a metal mesh (325 mesh) and poured into a feed liquid tank. During spinning, the core liquid flow rate was set to 1 mL / min, the feed liquid flow rate was set to 3 mL / min, the core liquid was a mixture solution of deionized water and NMP (15 / 85 wt.%), and the external coagulation bath was deionized water. The spun hollow fiber membrane was soaked in 85 wt.% methanol for 30 min, repeated 3 times, then moved to n-hexane and soaked for 30 min, repeated 3 times, and finally dried in a vacuum oven at 120 ° C for 24 h to obtain a PI-PIL (10:1) hollow fiber membrane.
[0066] Embodiment 2:
[0067] The difference from Example 1 is that in step (2), the amount of 1-vinyl-3-methylimidazolium iodide added is 1.0 g, and a PI-PIL (5:1) hollow fiber membrane is obtained.
[0068] Embodiment 3:
[0069] The difference from Example 1 is that in step (2), the amount of 1-vinyl-3-methylimidazolium iodide added is 2.5 g, and a PI-PIL (2:1) hollow fiber membrane is obtained.
[0070] Comparative Example:
[0071] The difference from Example 1 is that steps (1) and (2) are not performed, and in step (3), the polymer in the spinning solution is a polyimide resin (PI), and a PI hollow fiber membrane is obtained.
[0072] Test Example
[0073] (1) Infrared test of the resin obtained in the comparative example and the embodiment:
[0074] like Figure 1 , 1784cm -1 、1726cm -1 、1375cm -1 、1253cm -1 The characteristic absorption peak of the imide ring is 1649 cm -1 is the stretching vibration peak of C=C on the imidazole ring of the polyionic liquid, 1566cm -1 It is the stretching vibration peak of C=N on the imidazole ring of the polyionic liquid. And it can be clearly found that with the increase of the feeding amount of 1-vinyl-3-methylimidazolium iodide, the intensity of these two absorption peaks increases significantly.
[0075] (2) Molecular weight determination of the resins obtained in the embodiments and comparative examples:
[0076] The determination was performed using a gel permeation chromatograph, with DMF being the eluent at a flow rate of 1 mL / min.
[0077] Table 1 GPC test results of the resins obtained in the examples and comparative examples
[0078]
[0079] The results of the GPC test show that as the amount of 1-vinyl-3-methylimidazolium iodide added increases, the GPC results also increase, which indicates that the molecular weight of the polyionic liquid side chain increases with the increase in the amount of added.
[0080] (3) Inner and outer diameters of the hollow fiber membranes obtained in the examples and comparative examples:
[0081] Table 2 Comparison of the inner and outer diameters of the hollow fiber membranes obtained in the examples and comparative examples
[0082]
[0083] (4) Pure gas separation performance of the hollow fiber gas separation membranes obtained in the examples and comparative examples:
[0084] See Table 3, the test pressure is 0.5MPa and the test temperature is 35℃.
[0085] Table 3 Comparison of pure gas separation performance of hollow fiber membranes obtained in Examples and Comparative Examples
[0086]
[0087] From the pure gas separation performance test results, it can be seen that when the inner and outer diameters of the hollow fiber are similar, the polyimide gas separation membrane with a polyionic liquid side chain structure has a greatly improved selectivity for CO2 compared to the unmodified polyimide gas separation membrane. By comparing the three examples, it can be found that from PI-PIL (10:1) to PI-PIL (2:1), the permeability of the sample to CO2 gradually increases. This is because as the content of the polyionic liquid increases, the microphase separation phenomenon of the material becomes increasingly obvious, and the number of channels through which the gas can pass increases.
[0088] (5) Determination of thermal stability of hollow fiber membrane:
[0089] The measurement was performed using a thermogravimetric analyzer under a N2 atmosphere at a heating rate of 10 K / min.
[0090] according to Figure 4 The thermogravimetric test results show that the samples T d5% All of them exceed 300℃ and have good thermal stability.
[0091] (6) Determination of tensile strength and elongation at break of hollow fiber membranes:
[0092] The measurement was carried out using an electronic universal testing machine, with an effective sample length of 50 mm and a tensile rate of 2 mm / min.
[0093] according to Figure 5 The tensile test results show that the introduction of polyionic liquid side chains will lead to a decrease in the interaction force between polyimide molecular chains, which in turn leads to a decrease in tensile strength. However, there is not much difference between samples with different side chain lengths, and all have a strength of about 20MPa, which can meet the actual needs of gas separation.
[0094] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A polyimide hollow fiber membrane having a polyionic liquid side chain structure, characterized in that: It includes a polyimide main chain containing an alkyl group and a vinyl polyionic liquid side chain.
2. The method for preparing the polyimide hollow fiber membrane having a polyionic liquid side chain structure according to claim 1, characterized in that: The following steps are involved: (1) Under the protection of an inert atmosphere, a polyimide resin containing an alkyl structure, N-bromosuccinimide, and azobisisobutyronitrile are dissolved in an organic solvent, heated and stirred for reaction, and after the reaction is completed, the solution is poured into methanol for precipitation, and the obtained solid is a brominated polyimide resin; (2) Under the protection of an inert atmosphere, a brominated polyimide resin, a vinyl ionic liquid monomer, a catalyst, and a ligand are dissolved in an organic solvent, heated and stirred to react, and after the reaction is completed, the solution is poured into methanol for precipitation, and the resulting solid is a polyimide resin having a polyionic liquid side chain structure; (3) The polyimide resin having a polyionic liquid side chain structure is dissolved in an organic solvent, and the hollow fiber membrane is obtained by filtering, spinning, soaking and drying.
3. The method for preparing the polyimide hollow fiber membrane having a polyionic liquid side chain structure according to claim 1, characterized in that: The number average molecular weight of the polyimide resin containing an alkyl structure in step (1) is 1000 to 500000; The organic solvent in step (1) is one or more of chloroform, o-cresol, m-cresol, p-cresol, dimethyl sulfoxide, N-methylpyrrolidone, N,N-dimethylformamide and N,N-dimethylacetamide.
4. The method for preparing a polyimide hollow fiber membrane having a polyionic liquid side chain structure according to claim 1, characterized in that: In step (1), the mass ratio of the polyimide resin containing an alkyl structure, N-bromosuccinimide, and azobisisobutyronitrile is 100:(0.2-50):(0.001-0.5); the amount ratio of the polyimide resin containing an alkyl structure to the organic solvent is 1 g:(1-50) mL; The reaction temperature of step (1) is 30-70°C and the reaction time is 12-48h.
5. The method for preparing the polyimide hollow fiber membrane having a polyionic liquid side chain structure according to claim 1, characterized in that: The vinyl ionic liquid monomer in step (2) is at least one of the following compounds: Wherein, X is Cl, Br, I, COO, SCN, NO3, BF4 or PF6; The catalyst in step (2) is a transition metal halide; preferably one of CuCl, CuBr and CuI; The ligand in step (2) is one of the following compounds: The organic solvent in step (2) is one or more of dimethyl sulfoxide, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
6. The method for preparing the polyimide hollow fiber membrane having a polyionic liquid side chain structure according to claim 1, characterized in that: In step (2), the mass ratio of the brominated polyimide resin, the vinyl ionic liquid monomer, the catalyst, and the ligand is 100:(1-100):(0.01-0.5):(0.02-1); the amount ratio of the brominated polyimide resin to the organic solvent is 100 g:(100-5000) mL; The reaction temperature in step (2) is 60 to 120° C. and the reaction time is 12 to 36 hours. The number average molecular weight of the polyimide resin having a polyionic liquid side chain structure obtained in step (2) is 5,000 to 1,000,000.
7. The method for preparing the polyimide hollow fiber membrane having a polyionic liquid side chain structure according to claim 1, characterized in that: The organic solvent in step (3) is one or more of tetrahydrofuran, dimethyl sulfoxide, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide; The amount of the organic solvent in step (3) is such that the concentration of the polyimide resin having a polyionic liquid side chain structure in the spinning solution is 10 to 45 wt.%; The mesh size of the filtration in step (3) is 300 to 500.
8. The method for preparing the polyimide hollow fiber membrane having a polyionic liquid side chain structure according to claim 1, characterized in that: The spinning liquid in step (3) is the polyimide resin solution obtained after filtration, and the flow rate is 1-15 mL / min; the core liquid is a mixed solution of water and an organic solvent, and the flow rate is 0.2-5 mL / min, wherein the mass ratio of water to organic solvent is 50:50-10:90; The coagulation bath for spinning in step (3) is water; The hollow fiber membrane in step (3) has an outer diameter of 200 to 500 μm, an inner diameter of 150 to 350 μm, and a membrane thickness of 40 to 100 μm.
9. Use of the polyimide hollow fiber membrane having a polyionic liquid side chain structure as claimed in claim 1 in gas separation.
10. The use of the polyimide hollow fiber membrane having a polyionic liquid side chain structure in gas separation according to claim 9, characterized in that: The gas separation is to capture carbon dioxide from air, industrial flue gas, natural gas or biogas.
Citation Information
Patent Citations
Gas separation membranes and processes for the manufacture thereof
CN101910314A
Ionic liquid / polymer electrolyte membrane and preparation method thereof
CN104140545A
Polyionic liquid functionalized charged composite film and production method thereof
CN104707487A
Polymer membrane whereby ionic liquid functional groups are introduced in polymer side chains and manufacturing method thereof
KR1020140100048A