Preparation method of soft hollow water purification fiber
By preparing soft hollow water purification fibers and utilizing the hollow pore structure and high photocatalytic activity of gallium-titanium-gadolinium ternary composite oxide materials, the problem of insufficient catalytic activity and powder material separation in the treatment of organic pollutants in water is solved, achieving Efficient water treatment and convenient material separation.
Patent Information
- Application Number
- CN202410767844.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
AI Technical Summary
When the existing technology treats organic pollutants in water, the photocatalytic activity of the catalytic material is insufficient, and the separation of the powder material and water is difficult to achieve, which affects the treatment efficiency and continuous use.
Using the preparation method of soft hollow water purification fibers, a gallium-titanium-gadolinium ternary composite oxide material with a hollow pore structure was prepared through carbon fiber activation, gel coating and heat treatment of gallium-titanium-gadolinium ternary composite sol. , improve photocatalytic activity and facilitate separation from water.
Efficient treatment of organic pollutants in water is achieved. The material has a low density and stable structure, can be fully mixed with water, improves treatment efficiency, and is easy to separate after treatment, supporting continuous use.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of water pollution purification materials, and in particular relates to a method for preparing a soft hollow water purification fiber. Background Art
[0002] Industrial and civil wastewater contains a large amount of organic matter, and these organic matter are of various types, which poses a huge potential hazard to the ecological environment and human health. These wastewaters containing a large amount of pollutants must be strictly treated before being discharged into environmental water bodies, and can only be discharged after meeting the national control emission standards. The main method of water treatment is conventional biochemical treatment, but the microorganisms relied on by biochemical treatment lack sufficient adaptability and treatment capabilities for toxic substances. After half a century of in-depth research and development, photocatalytic oxidation technology has become a key technology that can replace biochemical oxidation, because photocatalytic oxidation can be used to treat most organic pollutants, including toxic and high-concentration organic substances.
[0003] The key to photocatalytic technology for treating pollution lies in the catalytic materials used. In addition to having sufficient treatment activity, the catalytic materials must also adapt to various complex sewage treatment conditions and meet specific treatment process requirements. Powder materials usually have high photocatalytic activity, but the separation of powder and water is a difficult problem to solve. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention aims to provide a method for preparing a soft hollow water purification fiber, which can be used in the photocatalytic oxidation purification process of organic pollutants in water.
[0005] The technical solution adopted by the present invention is:
[0006] A method for preparing a soft hollow water purification fiber comprises the following process steps:
[0007] Step 1: Activation of carbon fiber
[0008] (1) Put 3g of carbon fiber into a 500mL beaker, add 380mL of 0.5mol / L hydrochloric acid solution, soak for 30min, take out, rinse with pure water for later use;
[0009] (2) placing the washed carbon fiber in an oven at 120°C for 10 hours, and then placing it in a program-controlled electric furnace at 300°C for 2 hours to obtain activated carbon fiber;
[0010] Step 2: Preparation of Gallium-Titanium-Gadolinium Ternary Composite Sol
[0011] (1) Add 120-160 mL of anhydrous ethanol, 15-18 mL of butanediol, and 7.2-8.6 mL of n-butyl titanate into a beaker, and stir evenly to obtain a precursor A;
[0012] (2) In another beaker, add 30-35 mL of anhydrous ethanol, 5-6 g of polyethylene glycol with a molecular weight of 6000, 3.2-3.5 g of emulsifier Tween 60, 17.8-19.3 mL of pure water, 2.6-3.2 g of gallium nitrate and 4.5-5.1 g of gadolinium nitrate, and stir well to obtain precursor B;
[0013] (3) Precursor B is slowly added to precursor A, placed in a constant temperature water bath at 50° C., and stirred evenly to obtain a gallium-titanium-gadolinium ternary composite sol;
[0014] Step 3: Gel Coating
[0015] (1) adding the activated carbon fiber to the gallium-titanium-gadolinium ternary composite sol, stirring thoroughly, pulling out the activated carbon fiber coated with the gallium-titanium-gadolinium ternary composite sol and letting it stand for 1 hour;
[0016] (2) placing the activated carbon fiber coated with the sol in a -35°C freeze dryer for 12 hours to obtain gel-coated carbon fiber;
[0017] Step 4: Heat Treatment
[0018] The gel-coated carbon fiber is calcined in a program-controlled box-type electric furnace at 590-630° C. for 3.5 hours and then cooled to room temperature to obtain a soft hollow water purification fiber material.
[0019] Furthermore, the carbon fiber in step 1 has a diameter of 1 μm and a length of 10 cm.
[0020] A soft hollow water purification fiber is prepared by the above method. The hollow pore diameter of the soft hollow water purification fiber is 0.7-0.8 μm and the temperature resistance range is lower than 580°C.
[0021] Furthermore, the soft hollow water purification fiber material is mainly composed of gallium-titanium-gadolinium ternary composite oxide, which is a composite of three oxides: gallium oxide, titanium oxide and gadolinium oxide.
[0022] Compared with the prior art, the method for preparing a soft hollow water purification fiber of the present invention has the following advantages:
[0023] The present invention prepares a soft hollow water purification fiber material with gallium-titanium-gadolinium ternary composite oxide as the main component. The material has a hollow pore structure, so it has a low density, can be fully mixed with water during use to increase the treatment efficiency, and can be quickly separated from water after the water treatment process to achieve the purpose of continuous use. The gallium-titanium-gadolinium ternary composite oxide is composed of three oxides of gallium oxide, titanium oxide and gadolinium oxide. The relative proportions of the three oxides are scientifically combined and optimized, so this gallium-titanium-gadolinium ternary composite oxide has strong photocatalytic treatment activity and is easy to form a soft hollow water purification fiber with a stable structure. The preparation method in the present invention, such as the activation step of the carbon fiber and the gel coating step, is of great significance for preparing stable and highly active soft hollow water purification fibers. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0025] Example 1
[0026] A method for preparing a soft hollow water purification fiber comprises the following process steps:
[0027] Step 1: Activation of carbon fiber
[0028] (1) Put 3g of carbon fiber into a 500mL beaker, add 380mL of 0.5mol / L hydrochloric acid solution, soak for 30min, take out, rinse with pure water for later use;
[0029] (2) The washed carbon fiber is placed in an oven at 120°C for 10 hours, and then placed in a programmable electric furnace at 300°C for 2 hours to obtain activated carbon fiber.
[0030] Step 2: Preparation of Gallium-Titanium-Gadolinium Ternary Composite Sol
[0031] (1) Add 120 mL of anhydrous ethanol, 15 mL of butanediol, and 7.2 mL of n-butyl titanate into a beaker in sequence and stir evenly to obtain precursor A;
[0032] (2) In another beaker, add 30 mL of anhydrous ethanol, 5 g of polyethylene glycol with a molecular weight of 6000, 3.2 g of emulsifier Tween 60, 17.8 mL of pure water, 2.6 g of gallium nitrate and 4.5 g of gadolinium nitrate, and stir well to obtain precursor B.
[0033] (3) Precursor B is slowly added to precursor A, placed in a constant temperature water bath at 50° C., and stirred evenly to obtain a gallium-titanium-gadolinium ternary composite sol.
[0034] Step 3: Gel Coating
[0035] (1) adding activated carbon fiber to the gallium-titanium-gadolinium ternary composite sol, stirring thoroughly, pulling out the activated carbon fiber coated with the gallium-titanium-gadolinium ternary composite sol and letting it stand for 1 hour;
[0036] (2) The activated carbon fiber coated with the sol was placed in a -35°C freeze dryer for 12 hours to obtain gel-coated carbon fiber.
[0037] Step 4: Heat Treatment
[0038] The gel-coated carbon fiber was calcined in a program-controlled box-type electric furnace at 590° C. for 3.5 hours and then cooled to room temperature to obtain a soft hollow water purification fiber material.
[0039] Example 2
[0040] A method for preparing a soft hollow water purification fiber comprises the following process steps:
[0041] Step 1: Activation of carbon fiber
[0042] (1) Put 3g of carbon fiber into a 500mL beaker, add 380mL of 0.5mol / L hydrochloric acid solution, soak for 30min, take out, rinse with pure water for later use;
[0043] (2) The washed carbon fiber is placed in an oven at 120°C for 10 hours, and then placed in a programmable electric furnace at 300°C for 2 hours to obtain activated carbon fiber.
[0044] Step 2: Preparation of Gallium-Titanium-Gadolinium Ternary Composite Sol
[0045] (1) Add 130 mL of anhydrous ethanol, 16 mL of butanediol, and 7.5 mL of n-butyl titanate into a beaker in sequence and stir evenly to obtain precursor A;
[0046] (2) In another beaker, add 31 mL of anhydrous ethanol, 5.3 g of polyethylene glycol with a molecular weight of 6000, 3.3 g of emulsifier Tween 60, 18.2 mL of pure water, 2.7 g of gallium nitrate and 4.6 g of gadolinium nitrate, and stir well to obtain precursor B.
[0047] (3) Precursor B is slowly added to precursor A, placed in a constant temperature water bath at 50° C., and stirred evenly to obtain a gallium-titanium-gadolinium ternary composite sol.
[0048] Step 3: Gel Coating
[0049] (1) adding activated carbon fiber to the gallium-titanium-gadolinium ternary composite sol, stirring thoroughly, pulling out the activated carbon fiber coated with the gallium-titanium-gadolinium ternary composite sol and letting it stand for 1 hour;
[0050] (2) The activated carbon fiber coated with the sol was placed in a -35°C freeze dryer for 12 hours to obtain gel-coated carbon fiber.
[0051] Step 4: Heat Treatment
[0052] The gel-coated carbon fiber was calcined in a 600° C. program-controlled box-type electric furnace for 3.5 hours and then cooled to room temperature to obtain a soft hollow water purification fiber material.
[0053] Example 3
[0054] A method for preparing a soft hollow water purification fiber comprises the following process steps:
[0055] Step 1: Activation of carbon fiber
[0056] (1) Put 3g of carbon fiber into a 500mL beaker, add 380mL of 0.5mol / L hydrochloric acid solution, soak for 30min, take out, rinse with pure water for later use;
[0057] (2) The washed carbon fiber is placed in an oven at 120°C for 10 hours, and then placed in a programmable electric furnace at 300°C for 2 hours to obtain activated carbon fiber.
[0058] Step 2: Preparation of Gallium-Titanium-Gadolinium Ternary Composite Sol
[0059] (1) Add 140 mL of anhydrous ethanol, 16 mL of butanediol, and 7.7 mL of n-butyl titanate into a beaker in sequence and stir evenly to obtain precursor A;
[0060] (2) In another beaker, add 32 mL of anhydrous ethanol, 5.5 g of polyethylene glycol with a molecular weight of 6000, 3.3 g of emulsifier Tween 60, 18.6 mL of pure water, 2.9 g of gallium nitrate and 4.8 g of gadolinium nitrate, and stir well to obtain precursor B.
[0061] (3) Precursor B is slowly added to precursor A, placed in a constant temperature water bath at 50° C., and stirred evenly to obtain a gallium-titanium-gadolinium ternary composite sol.
[0062] Step 3: Gel Coating
[0063] (1) adding activated carbon fiber to the gallium-titanium-gadolinium ternary composite sol, stirring thoroughly, pulling out the activated carbon fiber coated with the gallium-titanium-gadolinium ternary composite sol and letting it stand for 1 hour;
[0064] (2) The activated carbon fiber coated with the sol was placed in a -35°C freeze dryer for 12 hours to obtain gel-coated carbon fiber.
[0065] Step 4: Heat Treatment
[0066] The gel-coated carbon fiber was calcined in a program-controlled box-type electric furnace at 610° C. for 3.5 hours and then cooled to room temperature to obtain a soft hollow water purification fiber material.
[0067] Example 4
[0068] A method for preparing a soft hollow water purification fiber comprises the following process steps:
[0069] Step 1: Activation of carbon fiber
[0070] (1) Put 3g of carbon fiber into a 500mL beaker, add 380mL of 0.5mol / L hydrochloric acid solution, soak for 30min, take out, rinse with pure water for later use;
[0071] (2) The washed carbon fiber is placed in an oven at 120°C for 10 hours, and then placed in a programmable electric furnace at 300°C for 2 hours to obtain activated carbon fiber.
[0072] Step 2: Preparation of Gallium-Titanium-Gadolinium Ternary Composite Sol
[0073] (1) Add 150 mL of anhydrous ethanol, 17 mL of butanediol, and 8.2 mL of n-butyl titanate into a beaker in sequence and stir evenly to obtain precursor A;
[0074] (2) In another beaker, add 33 mL of anhydrous ethanol, 5.7 g of polyethylene glycol with a molecular weight of 6000, 3.4 g of emulsifier Tween 60, 18.9 mL of pure water, 3.1 g of gallium nitrate and 4.9 g of gadolinium nitrate, and stir well to obtain precursor B.
[0075] (3) Precursor B is slowly added to precursor A, placed in a constant temperature water bath at 50° C., and stirred evenly to obtain a gallium-titanium-gadolinium ternary composite sol.
[0076] Step 3: Gel Coating
[0077] (1) adding activated carbon fiber to the gallium-titanium-gadolinium ternary composite sol, stirring thoroughly, pulling out the activated carbon fiber coated with the gallium-titanium-gadolinium ternary composite sol and letting it stand for 1 hour;
[0078] (2) The activated carbon fiber coated with the sol was placed in a -35°C freeze dryer for 12 hours to obtain gel-coated carbon fiber.
[0079] Step 4: Heat Treatment
[0080] The gel-coated carbon fiber was calcined in a program-controlled box-type electric furnace at 620° C. for 3.5 hours and then cooled to room temperature to obtain a soft hollow water purification fiber material.
[0081] Example 5
[0082] A method for preparing a soft hollow water purification fiber comprises the following process steps:
[0083] Step 1: Activation of carbon fiber
[0084] (1) Put 3g of carbon fiber into a 500mL beaker, add 380mL of 0.5mol / L hydrochloric acid solution, soak for 30min, take out, rinse with pure water for later use;
[0085] (2) The washed carbon fiber is placed in an oven at 120°C for 10 hours, and then placed in a programmable electric furnace at 300°C for 2 hours to obtain activated carbon fiber.
[0086] Step 2: Preparation of Gallium-Titanium-Gadolinium Ternary Composite Sol
[0087] (1) Add 160 mL of anhydrous ethanol, 18 mL of butanediol, and 8.6 mL of n-butyl titanate into a beaker in sequence and stir evenly to obtain precursor A;
[0088] (2) In another beaker, add 35 mL of anhydrous ethanol, 6 g of polyethylene glycol with a molecular weight of 6000, 3.5 g of emulsifier Tween 60, 19.3 mL of pure water, 3.2 g of gallium nitrate and 5.1 g of gadolinium nitrate, and stir well to obtain precursor B.
[0089] (3) Precursor B is slowly added to precursor A, placed in a constant temperature water bath at 50° C., and stirred evenly to obtain a gallium-titanium-gadolinium ternary composite sol.
[0090] Step 3: Gel Coating
[0091] (1) adding activated carbon fiber to the gallium-titanium-gadolinium ternary composite sol, stirring thoroughly, pulling out the activated carbon fiber coated with the gallium-titanium-gadolinium ternary composite sol and letting it stand for 1 hour;
[0092] (2) The activated carbon fiber coated with the sol was placed in a -35°C freeze dryer for 12 hours to obtain gel-coated carbon fiber.
[0093] Step 4: Heat Treatment
[0094] The gel-coated carbon fiber was calcined in a program-controlled box-type electric furnace at 630° C. for 3.5 hours and then cooled to room temperature to obtain a soft hollow water purification fiber material.
Claims
1. A method for preparing a soft hollow water purification fiber, characterized in that: The process includes the following steps: Step 1: Activation of carbon fiber (1) Put 3g of carbon fiber into a 500mL beaker, add 380mL of 0.5mol / L hydrochloric acid solution, soak for 30min, take out, rinse with pure water for later use; (2) placing the washed carbon fiber in an oven at 120°C for 10 hours, and then placing it in a program-controlled electric furnace at 300°C for 2 hours to obtain activated carbon fiber; Step 2: Preparation of Gallium-Titanium-Gadolinium Ternary Composite Sol (1) Add 120-160 mL of anhydrous ethanol, 15-18 mL of butanediol, and 7.2-8.6 mL of n-butyl titanate into a beaker, and stir evenly to obtain a precursor A; (2) In another beaker, add 30-35 mL of anhydrous ethanol, 5-6 g of polyethylene glycol with a molecular weight of 6000, 3.2-3.5 g of emulsifier Tween 60, 17.8-19.3 mL of pure water, 2.6-3.2 g of gallium nitrate and 4.5-5.1 g of gadolinium nitrate, and stir well to obtain precursor B; (3) Precursor B is slowly added to precursor A, placed in a constant temperature water bath at 50° C., and stirred evenly to obtain a gallium-titanium-gadolinium ternary composite sol; Step 3: Gel Coating (1) adding the activated carbon fiber to the gallium-titanium-gadolinium ternary composite sol, stirring thoroughly, pulling out the activated carbon fiber coated with the gallium-titanium-gadolinium ternary composite sol and letting it stand for 1 hour; (2) placing the activated carbon fiber coated with the sol in a -35°C freeze dryer for 12 hours to obtain gel-coated carbon fiber; Step 4: Heat Treatment The gel-coated carbon fiber is calcined in a program-controlled box-type electric furnace at 590-630° C. for 3.5 hours and then cooled to room temperature to obtain a soft hollow water purification fiber material.
2. The method for preparing a soft hollow water purification fiber according to claim 1, characterized in that: The carbon fiber in step 1 has a diameter of 1 μm and a length of 10 cm.
3. A soft hollow water purification fiber, prepared by the method of claim 1 or 2, characterized in that: The hollow pore diameter of the soft hollow water purification fiber is 0.7-0.8 μm, and the temperature resistance range is lower than 580°C.
4. A soft hollow water purification fiber according to claim 3, characterized in that: The soft hollow water purification fiber material takes gallium-titanium-gadolinium ternary composite oxide as the main component and is composited from three oxides of gallium oxide, titanium oxide and gadolinium oxide.