Ruthenium-based catalyst for catalyzing selective hydrogen absorption of liquid organic hydrogen carrier and preparation method of ruthenium-based catalyst
The spherical Ru/α-Al2O3 catalyst prepared by ball milling method solves the problems of complex catalyst preparation and high cost, realizes rapid and selective hydrogen absorption reaction at low temperature, improves the performance against impurity gases, and solves the problems in the existing technology. The problem of insufficient catalyst performance.
Patent Information
- Application Number
- CN202410742755.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-01
AI Technical Summary
Existing catalysts have problems such as slow catalytic rate for selective hydrogen absorption in liquid organic hydrogen carriers (LOHC), complex preparation processes, high production costs, and poor poison resistance.
The ball milling method is used to prepare spherical Ru/α-Al2O3 catalyst. Ru nanoparticles with good dispersion are formed by mixing triruthenium dodecacarbonyl and α-Al2O3 pellets in a hydrogen atmosphere and used to catalyze alkylcarbazole liquid organic Selective hydrogen absorption reaction of hydrogen carrier in hydrogen-containing gas.
It achieves rapid selective hydrogen absorption reaction at low reaction temperature, simplifies the catalyst preparation process, reduces costs, and improves the selective hydrogen absorption performance against CO, CO2, CH4, and H2O.
Smart Images

Figure CN118719052A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysis and hydrogen storage, and specifically relates to a ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier and a preparation method thereof. Background Art
[0002] Hydrogen energy is a clean and renewable secondary energy source and will be one of the key components in the future energy structure. Hydrogen storage technology has always been a bottleneck problem in the development of hydrogen energy. The commonly used method of hydrogen storage and transportation is high-pressure hydrogen storage. The produced hydrogen is generally compressed to more than 20MPa before storage and transportation. However, large-scale long-distance storage and transportation is very costly and there are also safety risks.
[0003] Liquid organic hydrogen carrier (LOHC) is a hydrogen storage technology based on the hydrogen addition reaction and hydrogen elimination reaction of liquid organic matter. It is considered to be one of the most promising hydrogen storage technologies due to its high hydrogen storage capacity, high safety, high adaptability and high economy, and has developed rapidly in recent years.
[0004] Currently, most LOHC technologies require the use of high-purity hydrogen for hydrogenation reactions. However, the crude hydrogen produced by many hydrogen production technologies is of low purity. For example, the crude hydrogen produced by coal reforming and biogas reforming contains CO, CO2, CH4, and H2O (water vapor). The crude hydrogen products produced by water electrolysis and hydrogen produced as a by-product of the chlor-alkali industry contain H2O (water vapor). Therefore, these crude hydrogen products need to be dried and purified before being stored and transported using LOHC technology.
[0005] Theoretically, LOHC only reacts with H2 under hydrogenation conditions. However, if crude hydrogen can be directly stored in LOHC to achieve integrated hydrogen purification, storage and transportation, the complexity and cost of the device can be significantly reduced, which is conducive to the development of hydrogen storage technology and promotes the application of hydrogen energy.
[0006] Some researchers are also conducting related research. For example, Peter Wasserscheid et al. found that under the catalysis of Pd / Al2O3, dibenzyltoluene (DBT) can selectively react with H2 from a mixture of H2, CO, CO2, and CH4 to produce 18H-DBT (Int. J Hydrogen Energy 2019, 44, 31172); Yoichi Hoshimoto et al. found that under the catalysis of halogenated triphenylborane, 2-methylquinoline (Qin) can selectively react with H2 from a mixture of H2, CO, and CO2 to produce tetrahydroquinoline (4H-Qin) (Sci. Adv. 2022, 8, 189); Che Defu et al. found that under the catalysis of Ru / Al2O3, N-ethylcarbazole (NEC) can selectively react with H2 from a mixture of H2 and CH4 to produce dodecahydro-N-ethylcarbazole (12H-NEC) (Fuel 2023, 331, 125920). Among them, DBT, Qin and NEC are typical liquid organic hydrogen carriers LOHC.
[0007] However, the Pd content in the above-mentioned Pd / Al2O3 catalyst is 5% (mass ratio), which is expensive, and CO has a great influence on the catalytic activity of the Pd / Al2O3 catalyst (at 300°C, with the addition of 2% CO, the hydrogen absorption rate is only 23% of that under pure hydrogen conditions); the synthesis process of halogenated triphenylborane is complicated and costly, and it is difficult to put it into practical use in the short term; the Ru / Al2O3 catalyst has poor resistance to CO and CO2, and has poor selective hydrogen absorption performance for crude hydrogen from biogas (CO, CO2, CH4, H2O).
[0008] Patent application CN202410002990.6 discloses a liquid organic hydrogen carrier selective hydrogen absorption catalyst and its preparation method, however, it still uses the relatively expensive palladium-based catalyst Pd / Al2O3-C, and the organic carrier used is benzyltoluene, which has a high hydrogen release temperature, resulting in high overall cost. In summary, the overall performance of the current selective hydrogen absorption catalyst materials and catalytic solutions needs to be further improved and optimized.
[0009] In addition, there are generally two ways to prepare shaped catalysts at present. One is to prepare powder catalysts or catalyst precursors first, and then obtain shaped particles by granulation methods such as extrusion and rotation. The other is to prepare shaped particle catalysts directly on the shaped particle carrier by impregnation, vapor deposition, etc. However, the existing methods are relatively complicated. Summary of the invention
[0010] The present invention aims to provide a ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier and a preparation method thereof in order to solve the problems of slow LOHC selective hydrogen absorption catalytic rate, complex catalyst preparation process, high production cost and poor anti-poisoning ability.
[0011] The technical solution adopted to achieve the purpose of the present invention is: a ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier, the ruthenium-based catalyst is a spherical Ru / α-Al2O3 catalyst, which is prepared by mixing triruthenium dodecacarbonyl and α-Al2O3 pellets in proportion and ball milling under hydrogen atmosphere conditions, wherein the mass ratio of triruthenium dodecacarbonyl to α-Al2O3 pellets is 1:100-200.
[0012] Preferably, the diameter of the α-Al2O3 spheres of the present invention is 0.5 to 2 mm.
[0013] Preferably, the pressure of the hydrogen in the present invention is 2 to 10 bar, and the ball milling conditions are: firstly performing a ball milling at a rotation speed of 200 to 300 rpm, and then performing a secondary ball milling at a rotation speed of 400 to 500 rpm.
[0014] Preferably, the first ball milling of the present invention has a ball milling time of 1 to 3 h; and the second ball milling has a ball milling time of 2 to 4 h.
[0015] Preferably, the catalyst of the present invention is used to catalyze the selective hydrogen absorption reaction of a liquid organic hydrogen carrier on a hydrogen-containing gas, and the liquid organic hydrogen carrier is one or both of ethylcarbazole and propylcarbazole.
[0016] Preferably, the mass ratio of the catalyst to the liquid organic hydrogen carrier of the present invention is (0.25-0.5):1.
[0017] Preferably, the components of the hydrogen-containing gas of the present invention are H2, CO, CO2, CH4, and water vapor H2O, and their volume ratios are (76-100): (0-2): (0-17): (0-4): (0-1).
[0018] Preferably, the catalytic reaction temperature of the hydrogen absorption reaction of the present invention is 180-200° C., and the hydrogen partial pressure in the hydrogen-containing gas is 8-9 MPa.
[0019] The present invention provides a method for preparing a ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier, and the preparation steps are as follows: Ru3(CO) 12The mixture is mixed with α-Al2O3 balls and placed in a ball mill, which is then evacuated for leak detection and filled with hydrogen with a pressure of 2 to 10 bar. The ball mill is then milled once at a speed of 200 to 300 rpm using a planetary ball mill for 1 to 3 h, and then milled twice at a speed of 400 to 500 rpm for 2 to 4 h to obtain a spherical Ru / α-Al2O3 catalyst.
[0020] Compared with the prior art, the technical advantages of the present invention are: 1) The shaped catalyst provided by the present invention is prepared by ball milling, and the balls used for ball milling are also catalyst carriers. Compared with the traditional method, this method is simple to operate and does not require high temperature and a large amount of solvent.
[0021] 2) The present invention realizes for the first time that an alkyl carbazole-based liquid organic hydrogen carrier can selectively react with hydrogen in a mixed gas of H2, CO, CO2, CH4, and H2O (water vapor), and the reaction temperature is low and the hydrogen absorption reaction rate is fast.
[0022] 3) The present invention uses triruthenium dodecacarbonyl as a precursor, which can be reduced under hydrogen ball milling conditions to form Ru nanoparticles with good dispersibility without introducing other impurities.
[0023] 4) The present invention ingeniously uses the technical solution of first low-intensity ball milling and then high-intensity ball milling, so that the precursor is first dispersed and then reduced, avoiding insufficient reduction of the precursor or agglomeration due to local high temperature during the ball milling process. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a physical picture of the Ru / α-Al2O3 catalyst prepared in Example 1 of the present invention.
[0025] Figure 2 This is a TEM image of Ru nanoparticles under ultrasound of the Ru / α-Al2O3 catalyst prepared in Example 1 of the present invention.
[0026] Figure 3 This is a hydrogen absorption curve of the spherical Ru / α-Al2O3 catalyst prepared in Example 1 of the present invention catalyzing the selective hydrogen absorption of NEPC (catalytic reaction temperature 190°C, hydrogen partial pressure 9 MPa, catalyst addition amount 25 wt%).
[0027] Figure 4 This is a chromatogram of hydrogen absorption products of NEPC selectively absorbed by the spherical Ru / α-Al2O3 catalyst prepared in Example 1 of the present invention (the retention time of 11-15 min is the full hydrogenation product, and the retention time of 15.5-17.5 min is the octahydrogenation product). DETAILED DESCRIPTION
[0028] The present invention will be further described below in conjunction with the embodiments.
[0029] The present invention discloses a ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier. The ruthenium-based catalyst is a spherical Ru / α-Al2O3 catalyst, which is prepared by mixing triruthenium dodecacarbonyl and α-Al2O3 pellets in proportion and ball milling under the condition of filling with hydrogen, wherein the mass ratio of the triruthenium dodecacarbonyl and the α-Al2O3 pellets is 1:100-200.
[0030] The diameter of the α-Al2O3 spheres is preferably 0.5 to 2 mm.
[0031] The preparation scheme of the ruthenium-based catalyst with selective hydrogen absorption is as follows: dodecacarbonyl triruthenium and α-Al2O3 balls are mixed and ball-milled in a certain proportion in a hydrogen atmosphere with a certain pressure, and the hydrogen pressure is 2 to 10 bar. The ball-milling is first carried out at a rotation speed of 200 to 300 rpm for 1 to 3 hours, and then at a rotation speed of 400 to 500 rpm for 2 to 4 hours to prepare a spherical Ru / α-Al2O3 catalyst.
[0032] The catalyst is used to catalyze the selective hydrogen absorption reaction of liquid organic hydrogen carrier to hydrogen-containing gas. The specific application is as follows: the prepared spherical Ru / α-Al2O3 catalyst is used to catalyze the selective hydrogen absorption reaction of liquid organic hydrogen carrier ethylcarbazole (or propylcarbazole, etc.) to hydrogen-containing gas, and the mass ratio of the spherical Ru / α-Al2O3 catalyst to the liquid organic hydrogen carrier is (0.25-0.5):1, and the spherical Ru / α-Al2O3 catalyst and the liquid organic hydrogen carrier are placed in a high-pressure reactor, the reactor is evacuated, the catalytic reaction temperature is set to 180-200°C, the stirring rate of the reactor is 300 rpm, the hydrogen partial pressure in the hydrogen-containing gas is 8-9 MPa, and the pressure change is detected by a pressure sensor after the gas is introduced. When the pressure no longer decreases, the reaction is stopped, and a liquid sample is taken for chromatographic analysis to obtain a hydrogen absorption curve. The hydrogen-containing gas composition is H2, CO, CO2, CH4, H2O (water vapor), and the volume ratio thereof is (76-100): (0-2): (0-17): (0-4): (0-1). Example 1
[0033] 10 gRu3(CO) 12 , 1000 g of α-Al2O3 balls with a diameter of 1 mm were mixed and placed in a ball mill, and then the ball mill was evacuated to check for leaks and filled with 10 bar of hydrogen. The ball mill was then milled at 300 rpm for 3 h and then at 500 rpm for 4 h using a planetary ball mill to obtain a spherical Ru / α-Al2O3 catalyst. The actual picture is as shown in the figure. Figure 1 .
[0034] The characterization results of inductively coupled plasma optical emission spectroscopy (ICP-OES) showed that the Ru loading in the spherical Ru / α-Al2O3 catalyst was 0.35 wt%, and the specific surface area of the spherical Ru / α-Al2O3 catalyst measured by nitrogen adsorption-desorption test was 8.5 m 2 / g. The Ru / α-Al2O3 catalyst was ultrasonicated in anhydrous ethanol, and then a sample was taken for transmission electron microscopy. Figure 2 This is the TEM image of Ru nanoparticles under ultrasound of Ru / α-Al2O3 catalyst. The results show that the size of Ru nanoparticles is 2~6 nm.
[0035] 2.5 g of spherical Ru / α-Al2O3 catalyst and 10 g of a mixture of ethylcarbazole (NEC) and propylcarbazole (NPC) (NEPC for short) were placed in a high-pressure reactor. After vacuuming and leak detection, the reactor was heated to 190 °C. A certain amount of hydrogen-containing gas (hydrogen partial pressure of 9 MPa) was introduced under mechanical stirring at 300 rpm. The pressure change was detected by a pressure sensor. The reaction was stopped when the pressure no longer dropped. A liquid sample was taken for chromatographic analysis to obtain a hydrogen absorption curve.
[0036] Among them, high-purity hydrogen and four hydrogen-containing gases were tested (the volume ratio of H2, CO, CO2, CH4, and H2O in iH-0 is 94:2:0:4:0; the volume ratio of H2, CO, CO2, CH4, and H2O in iH-1 is 95.3:1.7:1:1:1; the volume ratio of H2, CO, CO2, CH4, and H2O in iH-2 is 92:2:2:4:0; the volume ratio of H2, CO, CO2, CH4, and H2O in iH-18 is 76:2:18:4:0), and their hydrogen absorption curves are shown in Figure 2. Figure 3 As shown, the liquid product chromatogram is as Figure 4 As shown, the results show that in all hydrogen-containing atmospheres, NEPC can almost completely absorb hydrogen to obtain a fully hydrogenated product (i.e., a dodecahydrogen product). However, when the CO2 content is high, the selective hydrogen absorption rate is significantly reduced (the hydrogen absorption rate is only 8% of that under pure hydrogen conditions), but low content of CO, CO2, CH4, and H2O (water vapor) do not have a great effect on the hydrogen absorption rate (the hydrogen absorption rates under the three crude hydrogen conditions of iH-0, iH-1, and iH-2 are 88%, 76%, and 49% of that under pure hydrogen conditions, respectively). This indicates that the spherical Ru / α-Al2O3 catalyst can efficiently catalyze NEPC to selectively absorb hydrogen from mixed gases with low impurity content, and the hydrogen absorption rate is not significantly reduced compared to pure hydrogen conditions. Example 2
[0037] 5 gRu3(CO) 12, 1000 g of α-Al2O3 balls with a diameter of 2 mm were mixed and placed in a ball mill, which was then evacuated for leak detection and filled with 5 bar of hydrogen. The ball mill was then milled at 200 rpm for 2 h and then at 400 rpm for 2 h using a planetary ball mill to obtain a spherical Ru / α-Al2O3 catalyst.
[0038] 5 g of Ru / α-Al2O3 spherical catalyst and 10 g of ethylcarbazole (NEC) were placed in a high-pressure reactor. After vacuuming and leak detection, the reactor was heated to 180 °C and a certain amount of hydrogen-containing gas (hydrogen partial pressure of 8 MPa) was introduced under mechanical stirring at 300 rpm. The hydrogen pressure change was detected by a pressure sensor. The reaction was stopped when the pressure no longer dropped, and a liquid sample was taken for chromatographic analysis to obtain a hydrogen absorption curve.
[0039] High-purity hydrogen and iH-1 (the volume ratio of H2, CO, CO2, CH4, and H2O is 95.3:1.7:1:1:1) were tested. The results showed that in both hydrogen-containing atmospheres, NEC could almost completely absorb hydrogen to obtain a fully hydrogenated product (i.e., a dodecahydrogen product). The hydrogen absorption rate under crude hydrogen conditions was 80% of that under pure hydrogen conditions, indicating that the spherical Ru / α-Al2O3 catalyst can efficiently catalyze NEC to selectively absorb hydrogen from mixed gases with low impurity content, and the hydrogen absorption rate is not significantly reduced compared with pure hydrogen conditions. Example 3
[0040] 5 gRu3(CO) 12 , 1000 g of α-Al2O3 balls with a diameter of 0.5 mm were mixed and placed in a ball mill, which was then evacuated for leak detection and filled with 2 bar of hydrogen. The ball mill was then ball milled at 300 rpm for 1 h and then at 450 rpm for 2 h using a planetary ball mill to obtain a spherical Ru / α-Al2O3 catalyst.
[0041] 5 g of Ru / α-Al2O3 spherical catalyst and 10 g of propylcarbazole (NPC) were placed in a high-pressure reactor. After vacuuming and leak detection, the reactor was heated to 200 °C and a certain amount of hydrogen-containing gas (hydrogen partial pressure was 9 MPa) was introduced under mechanical stirring at 300 rpm. The pressure change was detected by a pressure sensor. The reaction was stopped when the pressure no longer dropped, and a liquid sample was taken for chromatographic analysis to obtain a hydrogen absorption curve.
[0042] High-purity hydrogen and iH-1 (the volume ratio of H2, CO, CO2, CH4, and H2O is 95.3:1.7:1:1:1) were tested. The results showed that in both hydrogen-containing atmospheres, NPC could almost completely absorb hydrogen to obtain a fully hydrogenated product (i.e., a dodecahydrogen product). The hydrogen absorption rate under crude hydrogen conditions was 72% of that under pure hydrogen conditions, indicating that the spherical Ru / α-Al2O3 catalyst can efficiently catalyze the selective absorption of hydrogen by NPC from mixed gases with low impurity content, and the hydrogen absorption rate is not significantly reduced compared with that under pure hydrogen conditions.
[0043] Comparative Example 1
[0044] 1 g of ruthenium nitrosyl nitrate and 100 g of α-Al2O3 balls with a diameter of 1 mm were mixed and placed in a ball mill, which was then evacuated to check for leaks and filled with 10 bar of hydrogen. The ball mill was then milled at 300 rpm for 3 h and then at 500 rpm for 4 h using a planetary ball mill to obtain a spherical Ru / α-Al2O3 catalyst.
[0045] 2.5 g of Ru / α-Al2O3 spherical catalyst and 10 g of NEPC were placed in a high-pressure reactor. After vacuuming and leak detection, the reactor was heated to 190 °C and a certain amount of hydrogen-containing gas (hydrogen partial pressure was 9 MPa) was introduced under mechanical stirring at 300 rpm. The pressure change was detected by a pressure sensor. The reaction was stopped when the pressure no longer dropped, and a liquid sample was taken for chromatographic analysis to obtain a hydrogen absorption curve.
[0046] High-purity hydrogen and iH-1 (the volume ratio of H2, CO, CO2, CH4, and H2O was 95.3:1.7:1:1:1) were tested, and the results showed that both atmospheres absorbed almost no hydrogen, indicating that the Ru precursor ruthenium nitrosyl nitrate is not suitable for preparing Ru / α-Al2O3 catalysts using this method, and that elemental Ru nanoparticles may not have been obtained.
[0047] Comparative Example 2
[0048] 1 g of anhydrous ruthenium chloride and 100 g of α-Al2O3 balls with a diameter of 1 mm were mixed and placed in a ball mill, which was then evacuated for leak detection and filled with 10 bar of hydrogen. The ball mill was then milled at 300 rpm for 3 h and then at 500 rpm for 4 h using a planetary ball mill to obtain a spherical Ru / α-Al2O3 catalyst.
[0049] 2.5 g of spherical Ru / α-Al2O3 catalyst and 10 g of NEPC were placed in a high-pressure reactor. After vacuuming and leak detection, the reactor was heated to 190 °C and a certain amount of hydrogen-containing gas (hydrogen partial pressure was 9 MPa) was introduced under mechanical stirring at 300 rpm. The pressure change was detected by a pressure sensor. The reaction was stopped when the pressure no longer dropped, and a liquid sample was taken for chromatographic analysis to obtain the hydrogen absorption curve.
[0050] High-purity hydrogen and iH-1 (the volume ratio of H2, CO, CO2, CH4, and H2O is 95.3:1.7:1:1:1) were tested. The results showed that both atmospheres absorbed almost no hydrogen, indicating that the Ru precursor sub-anhydrous ruthenium chloride is not suitable for preparing Ru / α-Al2O3 catalysts using this method, and elemental Ru nanoparticles may not have been obtained.
[0051] Comparative Example 3
[0052] 1 g Ru3(CO) 12 , 100 g of α-Al2O3 balls with a diameter of 1 mm were mixed and placed in a ball mill, which was then evacuated for leak detection and filled with 10 bar of hydrogen. The ball mill was then milled at 300 rpm for 7 h using a planetary ball mill to obtain a spherical Ru / α-Al2O3 catalyst.
[0053] A spherical 2.5 g Ru / α-Al2O3 catalyst and 10 g NEPC were placed in a high-pressure reactor. After vacuuming and leak detection, the reactor was heated to 190 °C and a certain amount of hydrogen-containing gas (hydrogen partial pressure was 9 MPa) was introduced under mechanical stirring at 300 rpm. The pressure change was detected by a pressure sensor. The reaction was stopped when the pressure no longer dropped, and a liquid sample was taken for chromatographic analysis to obtain a hydrogen absorption curve.
[0054] High-purity hydrogen and iH-1 (the volume ratio of H2, CO, CO2, CH4, and H2O was 95.3:1.7:1:1:1) were tested, and the results showed that both atmospheres absorbed almost no hydrogen, indicating that the ball milling speed of 300 rpm may not have produced elemental Ru nanoparticles.
[0055] Comparative Example 4
[0056] 1 g Ru3(CO) 12 , 100 g of α-Al2O3 balls with a diameter of 1 mm were mixed and placed in a ball mill, which was then evacuated for leak detection and filled with 10 bar of hydrogen. The ball mill was then milled at 400 rpm for 7 h using a planetary ball mill to obtain a spherical Ru / α-Al2O catalyst.
[0057] 2.5 g of spherical Ru / α-Al2O3 catalyst and 10 g of NEPC were placed in a high-pressure reactor. After vacuuming and leak detection, the reactor was heated to 190 °C and a certain amount of hydrogen-containing gas (hydrogen partial pressure was 9 MPa) was introduced under mechanical stirring at 300 rpm. The pressure change was detected by a pressure sensor. The reaction was stopped when the pressure no longer dropped, and a liquid sample was taken for chromatographic analysis to obtain the hydrogen absorption curve.
[0058] High-purity hydrogen and iH-1 (the volume ratio of H2, CO, CO2, CH4, and H2O is 95.3:1.7:1:1:1) were tested. The results showed that both atmospheres could selectively absorb hydrogen, but the hydrogen absorption rate was less than 30% of that in Example 1 under the same conditions, indicating that the ball milling speed of 400 rpm may not disperse Ru3(CO) well. 12 , resulting in larger single Ru nanoparticles with poor performance. Therefore, in Example 1, the precursor Ru3(CO) was first dispersed at a low speed. 12 , and then use the local high temperature generated by high speed to reduce the precursor Ru3(CO) with hydrogen 12 Obtaining Ru element is critical, because the hydrogen reduction of triruthenium dodecacarbonyl needs to be carried out at a certain temperature. During the ball milling process, due to collision, the local temperature will be very high, and the ball milling speed, time, etc. will affect this temperature. Therefore, appropriate ball milling intensity is required to reduce triruthenium dodecacarbonyl.
Claims
1. A ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier, characterized in that: The ruthenium-based catalyst is a spherical Ru / α-Al2O3 catalyst, which is prepared by mixing triruthenium dodecacarbonyl and α-Al2O3 pellets in proportion and ball milling under hydrogen atmosphere conditions, wherein the mass ratio of triruthenium dodecacarbonyl to α-Al2O3 pellets is 1:100-200.
2. The ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier according to claim 1, characterized in that: The diameter of the α-Al2O3 spheres is 0.5-2 mm.
3. The ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier according to claim 2, characterized in that: The pressure of the hydrogen is 2-10 bar, and the ball milling conditions are: firstly, ball milling is performed at a rotation speed of 200-300 rpm, and then, ball milling is performed twice at a rotation speed of 400-500 rpm.
4. The ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier according to claim 3, characterized in that: The first ball milling has a ball milling time of 1 to 3 hours; the second ball milling has a ball milling time of 2 to 4 hours.
5. The ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier according to claim 4, characterized in that: The catalyst is used for catalyzing the selective hydrogen absorption reaction of a liquid organic hydrogen carrier on a hydrogen-containing gas. The liquid organic hydrogen carrier is one or both of ethyl carbazole and propyl carbazole.
6. The ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier according to claim 5, characterized in that: The mass ratio of the catalyst to the liquid organic hydrogen carrier is (0.25-0.5):
1.
7. The ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier according to claim 5, characterized in that: The components of the hydrogen-containing gas are H2, CO, CO2, CH4, and water vapor H2O, and the volume ratios thereof are (76-100): (0-2): (0-17): (0-4): (0-1).
8. The ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier according to claim 7, characterized in that: The catalytic reaction temperature of the hydrogen absorption reaction is 180-200°C, and the hydrogen partial pressure in the hydrogen-containing gas is 8-9 MPa.
9. A method for preparing a ruthenium-based catalyst for catalyzing the selective hydrogen absorption of a liquid organic hydrogen carrier as claimed in claim 1 or 2, characterized in that: The preparation steps are as follows: Ru3(CO) 12 The mixture is mixed with α-Al2O3 balls and placed in a ball mill, which is then evacuated for leak detection and filled with hydrogen with a pressure of 2 to 10 bar. The ball mill is then milled once at a speed of 200 to 300 rpm using a planetary ball mill for 1 to 3 h, and then milled twice at a speed of 400 to 500 rpm for 2 to 4 h to obtain a spherical Ru / α-Al2O3 catalyst.