Bimetal oxide catalyst, solid hydrogen storage composite material, preparation method and application

By doping the Fe2TiO5 catalyst with MgH2, the problem of difficulty in reducing the MgH2 dehydrogenation activation energy is solved, more efficient hydrogen absorption and release kinetics are achieved, and the application potential of magnesium-based hydrogen storage materials is improved.

CN118719063APending Publication Date: 2024-10-01JIANGSU JICUI ANTAI CHUANGMING ADVANCED ENERGY MATERIALS RES INST CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410795351.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, the dehydrogenation activation energy of magnesium-based hydrogen storage material MgH2 is difficult to reduce below 100kJ/mol, which limits its application potential.

Method used

Fe2TiO5 is used as a bimetal oxide catalyst, which is prepared by hydrothermal treatment and calcination of urea, iron source and titanium source. The catalyst is doped with MgH2 in combination with the ball milling method to form an MgH2-Fe2TiO5 composite material to reduce its dehydrogenation activation energy.

Benefits of technology

It effectively reduces the dehydrogenation activation energy of MgH2 to 73.5-89.4kJ/mol, and significantly improves its hydrogen absorption and release kinetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719063A_ABST
    Figure CN118719063A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of magnesium-based solid hydrogen storage materials, in particular to a bimetallic oxide catalyst, a solid hydrogen storage composite material and a preparation method and application thereof.The bimetallic oxide catalyst comprises Fe2TiO5. The preparation method of the bimetallic oxide catalyst comprises the following steps that S1, urea is added into a solvent and stirred to be dissolved, then the mixture is heated to the reaction temperature, and a reaction solution is obtained; keeping constant temperature to obtain a constant-temperature solvent; s2, adding an iron source into a constant-temperature solvent, stirring until the iron source is dissolved, then adding a titanium source, and stirring until a full reaction; s3, carrying out hydro-thermal treatment on the solution after full reaction in the step S2, and carrying out post-treatment to obtain a catalyst precursor; and S4, calcining the catalyst precursor to obtain the bimetallic oxide catalyst. After the bimetallic oxide catalyst provided by the invention is applied to a magnesium-based hydrogen storage material, the dehydrogenation activation energy of MgH2 can be further reduced to 73.5-89.4 kJ / mol.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnesium-based solid hydrogen storage materials, and in particular to a bimetallic oxide catalyst, a solid hydrogen storage composite material, and a preparation method and application thereof. Background Art

[0002] The combustion of traditional fossil fuels has led to serious environmental pollution and has made the energy crisis a key issue in the development of the world today. The development of clean and sustainable new energy materials is imminent. Among new energy materials, hydrogen energy has attracted more and more attention due to its advantages such as high combustion calorific value, abundant resources and green and pollution-free. The production and storage technology of hydrogen has become the core issue that needs to be solved for the efficient development and utilization of hydrogen energy. The main methods of hydrogen storage are high-pressure gaseous hydrogen storage, liquid hydrogen storage and solid hydrogen storage technology. High-pressure gaseous hydrogen storage and liquid hydrogen storage are not suitable for large-scale application due to their poor safety and high cost, while solid hydrogen storage technology has attracted much attention due to its advantages such as high hydrogen storage density, high safety and easy transportation.

[0003] Among solid hydrogen storage materials, magnesium-based hydrogen storage materials (MgH2) have become a new energy material with great potential due to their abundant resources, low cost and high hydrogen storage capacity (7.6wt.%). However, their practical application is hindered by their slow hydrogen absorption and desorption rate and high initial dehydrogenation temperature (>400°C). At present, the main methods for modifying MgH2 include alloying, nano-sizing and catalyst doping. Among them, catalyst doping has an excellent effect on improving the kinetic rate of hydrogen absorption / desorption of MgH2. At the same time, the preparation of composite materials by doping catalysts and MgH2 by mechanical ball milling is simple to operate and has strong practicality, which can significantly enhance the hydrogen absorption / desorption kinetics of MgH2. In the prior art, bimetallic oxide catalysts based on Fe or Ti have certain improvements on the performance of magnesium-based solid hydrogen storage materials. For example, by adding 10wt.% LaFeO3 catalyst synthesized by solid-state method through ball milling process, the initial dehydrogenation temperature of MgH2 can be reduced by 120℃, and the dehydrogenation activation energy of MgH2 can be reduced to 107kJ / mol; adding 10wt.% CuFeO4 combined with Cu and Fe can also reduce the dehydrogenation activation energy of MgH2 from 166.0kJ / mol to 113.0kJ / mol; similarly, adding 3wt.% TiNb2O7 nanosheets can also effectively reduce the dehydrogenation activation energy of MgH2 to 100.4kJ / mol, so that the MgH2-3wt.% TiNb2O7 composite material has excellent hydrogen absorption and desorption performance.

[0004] Although bimetallic oxide catalysts based on Fe or Ti elements have improved the performance of magnesium-based hydrogen storage materials to a certain extent, the dehydrogenation activation energy of MgH2 is difficult to reduce to below 100 kJ / mol. Therefore, it is necessary to study a new magnesium-based hydrogen storage material catalyst to further reduce the dehydrogenation activation energy of MgH2. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a bimetallic oxide catalyst, a solid hydrogen storage composite material, and a preparation method and application. After the bimetallic oxide catalyst provided by the present invention is applied to a magnesium-based hydrogen storage material, the dehydrogenation activation energy of MgH2 can be further reduced to 73.5-89.4 kJ / mol.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a bimetallic oxide catalyst comprising Fe2TiO5.

[0008] After the bimetallic oxide catalyst provided by the present invention is applied to the magnesium-based hydrogen storage material, the dehydrogenation activation energy of MgH2 can be further reduced to 73.5-89.4 kJ / mol.

[0009] Further, the Fe2TiO5 is in a coral shape;

[0010] And / or, the Fe2TiO5 is a catalyst for magnesium-based hydrogen storage materials.

[0011] In a second aspect, the present invention provides a method for preparing the bimetallic oxide catalyst as described in the first aspect, the preparation method comprising the following steps:

[0012] S1, adding urea to the solvent and stirring until dissolved, then heating to the reaction temperature and maintaining a constant temperature to obtain a constant temperature solvent;

[0013] S2, adding an iron source to the constant temperature solvent obtained in step S1, stirring until the iron source is dissolved, and then adding a titanium source, stirring until the reaction is fully reacted;

[0014] S3, performing hydrothermal treatment on the solution after sufficient reaction in step S2, and obtaining a catalyst precursor after post-treatment;

[0015] S4, calcining the catalyst precursor obtained in step S3 to obtain the bimetallic oxide catalyst.

[0016] Further, in step S1, the solvent includes ethylene glycol;

[0017] and / or, in step S1, the mass ratio of the urea to the volume of the solvent is (0.02-0.04): 1 g / ml;

[0018] And / or, in step S1, the heating method is a water bath or an oil bath;

[0019] and / or, in step S1, the reaction temperature is 30-40°C;

[0020] and / or, the iron source comprises FeCl3·6H2O;

[0021] And / or, the mass ratio of the urea to the iron source is (1-3):3;

[0022] And / or, the titanium source includes tetrabutyl titanate, and the molar ratio of tetrabutyl titanate to FeCl3·6H2O is 1:1.

[0023] Furthermore, in step S2, the stirring time when the iron source is dissolved is 30-40 minutes;

[0024] and / or, in step S2, adding the titanium source dropwise;

[0025] And / or, in step S2, the stirring time until the reaction is fully completed is 4-5 hours;

[0026] And / or, the temperature of the hydrothermal treatment is 160-180°C;

[0027] And / or, the hydrothermal treatment time is 6-8h;

[0028] And / or, in step S3, the post-treatment includes filtering, washing and drying the product after the hydrothermal treatment, wherein the washing solvent includes ethanol, the drying temperature is 60-80° C., and the drying time is 10-12 h;

[0029] and / or, in step S4, the calcination temperature is 600-650°C;

[0030] And / or, in step S4, the calcination time is 1-2h;

[0031] And / or, in step S4, the calcination atmosphere is an air atmosphere.

[0032] In a third aspect, the present invention provides a solid hydrogen storage composite material, comprising MgH2 and a catalyst, wherein the catalyst is the catalyst described in the first aspect or a catalyst prepared by the preparation method described in the second aspect.

[0033] Further, the percentage of the catalyst in the solid hydrogen storage composite material is 3-10wt%;

[0034] And / or, the MgH2 is prepared by hydrogenation combustion synthesis.

[0035] In a fourth aspect, the present invention provides a method for preparing the solid hydrogen storage composite material as described in the third aspect, the preparation method comprising: adding the catalyst to the MgH2 according to a ratio, mixing them evenly by ball milling, and preparing the solid hydrogen storage composite material.

[0036] Furthermore, in the ball milling method, the ball milling mixing time is 8-12 hours, the ball-to-material ratio is 25-35:1, and the rotation speed is 300-500 r / min.

[0037] In a fifth aspect, the present invention provides a use of the solid hydrogen storage composite material as described in the third aspect or the solid hydrogen storage composite material prepared by the preparation method described in the fourth aspect in a product requiring hydrogen.

[0038] Compared with the prior art, the beneficial effects of the present invention include at least one of the following:

[0039] (1) After the bimetallic oxide catalyst provided by the present invention is applied to magnesium-based hydrogen storage materials, the activation energy of MgH2 dehydrogenation can be further reduced to 73.5-89.4 kJ / mol. (2) The present invention is the first to apply the Fe2TiO5 bimetallic oxide catalyst constructed by Fe and Ti elements to the catalytic modification research of MgH2, showing a catalytic effect better than that of single metal oxides. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0041] Figure 1 is the XRD pattern of the Fe2TiO5 catalyst prepared in Example 1 of the present invention;

[0042] Figure 2a is a SEM image of the Fe2TiO5 catalyst prepared in Example 1 of the present invention;

[0043] Figure 2b is a particle size distribution diagram of the Fe2TiO5 catalyst prepared in Example 1 of the present invention;

[0044] Figure 3aThis is a TEM image of the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention in a dehydrogenated state;

[0045] Figure 3b HRTEM and corresponding SAED images of the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention in a dehydrogenated state;

[0046] Figure 3c Another HRTEM image and corresponding SAED image of the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention in a dehydrogenated state;

[0047] Figure 3d TEM images of the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention in a dehydrogenated state and element mapping diagrams of Mg, Fe and Ti obtained by scanning different elemental components;

[0048] Figure 4a XPS spectra of Fe 2p in the dehydrogenated state and the hydrogenated state after 10 cycles of the Fe 2 TiO 5 catalyst prepared in Example 1 of the present invention and the MgH 2 -8 wt % Fe 2 TiO 5 sample;

[0049] Figure 4b XPS spectra of Ti 2p in the dehydrogenated state and the hydrogenated state after 10 cycles of the Fe2TiO5 catalyst and MgH2-8wt% Fe2TiO5 sample prepared in Example 1 of the present invention;

[0050] Figure 5 It is a comparison chart (5°C / min) of TPD curves of MgH2-8 wt% Fe, MgH2-8 wt% TiO2MgH2-8 wt% Fe2O3 prepared in Comparative Examples 1-3 of the present invention and the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 (first three times);

[0051] Figure 6a Isothermal hydrogenation curves (3MPa) of MgH2-8 wt%Fe2TiO5 prepared in Example 1 of the present invention at different temperatures;

[0052] Figure 6b The isothermal dehydrogenation curves (0.005 MPa) of MgH2-8 wt% Fe2TiO5 prepared in Example 1 of the present invention at different temperatures;

[0053] Figure 7a The kinetic curve of 10 hydrogen absorption and desorption cycles of the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention at 300°C;

[0054] Figure 7b The capacity curve of MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention after 10 cycles of hydrogen absorption and desorption at 300°C;

[0055] Figure 8a It is a fitting diagram of the dehydrogenation curve and the kinetic equation g(α) of the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention at different temperatures;

[0056] Figure 8b This is a diagram showing the calculation results of the dehydrogenation activation energy of the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0057] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0058] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0059] In a first aspect, the present invention provides a bimetallic oxide catalyst comprising Fe2TiO5.

[0060] After the bimetallic oxide catalyst provided by the present invention is applied to the magnesium-based hydrogen storage material, the dehydrogenation activation energy of MgH2 can be further reduced to 73.5-89.4 kJ / mol, preferably to 76.72 kJ / mol.

[0061] The Fe2TiO5 catalyst provided by the present invention has a "coral-like" morphology ( Figure 2a ), and the nanoparticles were observed to be connected at high magnification ( Figure 2b), with a large surface area; by introducing it into MgH2 for the first time by ball milling for catalytic modification research, the MgH2-Fe2TiO5 composite material can release about 6.17wt% H2 within 1000s at 300℃, and absorb about 5.89wt% H2 within 300s at 150℃. The activation energy of dehydrogenation of the composite material can be reduced to 76.72kJ / mol, which shows that the Fe2TiO5 catalyst effectively improves the hydrogen storage kinetics of MgH2. The reason can be found that the catalyst has a unique "coral-like" morphology, fully contacts with the MgH2 substrate during ball milling, and reacts with MgH2 during the first dehydrogenation to produce new phases: Fe, Fe2O3 and TiO2. The new phases generated in situ construct a multivalent and multi-element catalytic environment, forming more active catalytic sites on the MgH2 / Mg surface, providing a faster channel for the diffusion of H atoms during the absorption and release of H2, and finally the three complement each other to synergistically catalyze the absorption / desorption process of MgH2.

[0062] In the above-mentioned bimetallic oxide catalyst, as an optional embodiment, the Fe2TiO5 is in a coral shape.

[0063] In the above-mentioned bimetallic oxide catalyst, as an optional embodiment, the Fe2TiO5 is a catalyst for magnesium-based hydrogen storage materials.

[0064] In a second aspect, the present invention provides a method for preparing the bimetallic oxide catalyst as described in the first aspect, the preparation method comprising the following steps:

[0065] S1, adding urea to the solvent and stirring until dissolved, then heating to the reaction temperature and maintaining a constant temperature to obtain a constant temperature solvent;

[0066] S2, adding an iron source to the constant temperature solvent obtained in step S1, stirring until the iron source is dissolved, and then adding a titanium source, stirring until the reaction is fully reacted;

[0067] S3, performing hydrothermal treatment on the solution after sufficient reaction in step S2, and obtaining a catalyst precursor after post-treatment;

[0068] S4, calcining the catalyst precursor obtained in step S3 to obtain the bimetallic oxide catalyst.

[0069] In the present invention, the precursor formed after the hydrothermal treatment in step S3 contains organic components, and the organic components or other impurity phases can be removed by calcining at a high temperature in step S4.

[0070] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation, in step S1, the solvent includes ethylene glycol.

[0071] In the above-mentioned preparation method of the bimetallic oxide catalyst, as an optional implementation, in step S1, the volume ratio of the mass of the urea to the solvent is (0.02-0.04):1 g / ml, for example, it can be 0.02:1 g / ml, 0.03:1 g / ml or 0.04:1 g / ml.

[0072] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation, in step S1, the heating method is a water bath or an oil bath.

[0073] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation, in step S1, the reaction temperature is 30-40°C.

[0074] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation, the iron source includes FeCl3·6H2O.

[0075] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation, the mass ratio of the urea to the iron source is (1-3):3, for example, it can be 1:3, 2:3 or 3:3.

[0076] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation, the titanium source includes tetrabutyl titanate.

[0077] In order to ensure the physical purity of the prepared bimetallic oxide catalyst Fe2TiO5, in the above-mentioned preparation method of the bimetallic oxide catalyst, as an optional implementation, the molar ratio of tetrabutyl titanate and FeCl3·6H2O is 1:1.

[0078] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation, in step S2, the stirring time when stirring until the iron source is dissolved is 30-40 minutes.

[0079] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation, in step S2, the titanium source is added dropwise.

[0080] In the above-mentioned preparation method of the bimetallic oxide catalyst, as an optional implementation, in step S2, the stirring time until the reaction is fully achieved is 4-5 hours, and long-term stirring can ensure that the iron source and the titanium source react fully in the solvent.

[0081] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional embodiment, the temperature of the hydrothermal treatment is 160-180°C, for example, it can be 160°C, 165°C, 170°C, 175°C or 180°C.

[0082] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation manner, the hydrothermal treatment time is 6-8h.

[0083] In the above-mentioned preparation method of the bimetallic oxide catalyst, as an optional embodiment, in step S3, the post-treatment includes filtering, washing and drying the product after the hydrothermal treatment, wherein the washing solvent includes ethanol, the drying temperature is 60-80°C (for example, 60°C, 65°C, 70°C, 175°C or 180°C), and the time is 10-12h. The use of anhydrous ethanol solvent during washing can effectively remove the solvent and impurities on the surface of the hydrothermal product.

[0084] In the above-mentioned preparation method of the bimetallic oxide catalyst, as an optional embodiment, in step S4, the calcination temperature is 600-650° C., for example, 600° C., 610° C., 630° C. or 650° C. Too high a calcination temperature will carbonize the catalyst, while too low a calcination temperature will cause organic components to remain in the precursor, making the catalyst impure and reducing the catalytic performance.

[0085] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation, in step S4, the calcination time is 1-2 hours.

[0086] In the above-mentioned method for preparing the bimetallic oxide catalyst, as an optional implementation, in step S4, the calcination atmosphere is an air atmosphere.

[0087] In a third aspect, the present invention provides a solid hydrogen storage composite material, comprising MgH2 and a catalyst, wherein the catalyst is the catalyst described in the first aspect or a catalyst prepared by the preparation method described in the second aspect.

[0088] The composite material provided by the present invention generates a new phase in situ during the first dehydrogenation process. Compared with active doping, the in situ generated phase has a better catalytic effect, and a multivalent and multi-element catalytic environment is constructed in the composite system. The new phase synergistically catalyzes the hydrogen storage performance of MgH2. The present invention greatly reduces the dehydrogenation activation energy (76.72 kJ / mol) of MgH2 by introducing the Fe2TiO5 catalyst, and accelerates the hydrogen absorption and desorption kinetics of MgH2.

[0089] In the above-mentioned solid hydrogen storage composite material, as an optional embodiment, the percentage of the catalyst in the solid hydrogen storage composite material is 3-10wt%, for example, it can be 3wt%, 5wt%, 7wt% or 10wt%. If the catalyst content is too low, the catalytic effect is not significant. If the catalyst content is too high, the catalytic effect is significant, but the decrease in the MgH2 ratio will reduce the hydrogen storage capacity of the composite material, so 8wt% is preferred.

[0090] In the above-mentioned solid-state hydrogen storage composite material, as an optional implementation, the MgH2 is prepared by hydrogenation combustion synthesis (HCS).

[0091] In the above-mentioned solid hydrogen storage composite material, as an optional embodiment, the preparation method of MgH2 comprises the following steps:

[0092] The raw magnesium powder is placed in a reaction boat in a furnace chamber for reaction. In order to avoid the presence of impurity gases such as oxygen during the reaction, the furnace chamber pressure is first pumped to 25Pa by a vacuum pump and then filled with 0.2MPa argon for cleaning three times to ensure the purity of the gas in the furnace chamber. Subsequently, 2.0MPa hydrogen is filled in. Next, the furnace chamber is heated from room temperature to 580°C and then kept warm for 2h at a heating rate of 10°C / min. The heating system is then turned off and naturally cooled to 340°C and kept warm for 8h. The pressure can be adjusted during the reaction to always keep the hydrogen pressure at 2.0MPa. Finally, the heating and hydrogen input are stopped and naturally cooled to room temperature. Preferably, the raw magnesium powder does not need to be pre-milled or pressed.

[0093] In a fourth aspect, the present invention provides a method for preparing the solid hydrogen storage composite material as described in the third aspect, the preparation method comprising: adding the catalyst (Fe2TiO5) to the MgH2 according to a ratio, mixing them evenly by ball milling, and preparing the solid hydrogen storage composite material (MgH2-Fe2TiO5 composite material).

[0094] In the preparation method of the above-mentioned solid hydrogen storage composite material, as an optional implementation mode, in the ball milling method, the ball milling mixing time is 8-12h (for example, 8.5h, 9h, 10h, 11h, 11.5h), the ball-to-material ratio is 25-35:1 (for example, 26:1, 28:1, 30:1, 20:1, 32:1, 34:1), and the rotation speed is 300-500r / min (for example, 310r / min, 350r / min, 400r / min, 450r / min, 490r / min); preferably, the ball-to-material ratio is 30:1, the rotation speed is 400rpm, the ball milling is for 10 hours, and the working time is 30min and the stop time is 6min.

[0095] In a fifth aspect, the present invention provides a use of the solid hydrogen storage composite material as described in the third aspect or the solid hydrogen storage composite material prepared by the preparation method described in the fourth aspect in a product requiring hydrogen.

[0096] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0097] In the following examples and comparative examples:

[0098] Fe catalyst was purchased from MacLean Reagent Co., Ltd.

[0099] Fe2O3 catalyst was purchased from MacLean Reagent Co., Ltd.

[0100] Example 1

[0101] The bimetallic oxide catalyst provided in this embodiment is Fe2TiO5.

[0102] The preparation method of Fe2TiO5 comprises the following steps:

[0103] S1. Weigh 1.8 g of CO(NH2)2 particles, add them to 60 mL of ethylene glycol solvent, stir magnetically for 30 min, and after the particles are completely dissolved, heat the solution in a water bath to a constant temperature of 30 °C.

[0104] S2, add 2.7g FeCl3·6H2O to the water bath solution obtained in step S1, stir magnetically for 30min to obtain a uniform brown solution; use a pipette to measure 3.4mL Ti(OC4H9)4, add dropwise to the above brown solution and continue stirring for 4h;

[0105] S3, pour the mixed solution in S2 into a Teflon-lined container, put it into a high-pressure reactor, place it in a constant temperature oven at 160°C for hydrothermal treatment for 6 hours, filter and wash the hydrothermal product three times with anhydrous ethanol, and dry the product in a vacuum oven at 60°C for 12 hours to obtain a catalyst precursor (Fe2TiO5 precursor);

[0106] S4. In an air atmosphere, the dried Fe2TiO5 precursor was heated to 600°C at 5°C / min, calcined at 600°C for 2h, and then naturally cooled to room temperature to finally obtain brown Fe2TiO5 powder.

[0107] The solid hydrogen storage composite material provided in the present embodiment includes MgH2 and the bimetallic oxide catalyst Fe2TiO5 provided in the present embodiment, Fe2TiO5 accounts for 8wt% of the solid hydrogen storage composite material, and MgH2 accounts for 92wt% of the solid hydrogen storage composite material, wherein MgH2 is prepared by hydrogenation combustion synthesis (HCS). First, the raw magnesium powder is placed in a reaction boat in a furnace chamber for reaction. In order to avoid the presence of impurity gases such as oxygen during the reaction, the furnace chamber pressure is first evacuated to 25Pa by a vacuum pump and then filled with 0.2MPa argon gas for cleaning three times to ensure the purity of the gas in the furnace chamber, followed by filling with 2.0MPa hydrogen. Next, the Mg powder is heated from room temperature to 580°C and then kept warm for 2h at a heating rate of 10°C / min. Subsequently, the heating system is turned off and naturally cooled to 340°C and kept warm for 8h. During the reaction, the pressure can be adjusted to always keep the hydrogen pressure at 2.0MPa. Finally, the heating and hydrogen input are stopped, and the furnace chamber is naturally cooled to room temperature to obtain MgH2.

[0108] The preparation method of the solid hydrogen storage composite material provided in this embodiment includes: adding Fe2TiO5 to MgH2 prepared in this embodiment according to a mass percentage formula, and mixing by ball milling to obtain a MgH2-8 wt% Fe2TiO5 composite material; wherein the ball-to-material ratio is 30:1, the rotation speed is 400 rpm, the ball milling is 10 hours, and the work is stopped for 6 minutes every 30 minutes.

[0109] Example 2

[0110] The bimetallic oxide catalyst provided in this embodiment is Fe2TiO5.

[0111] The preparation method of Fe2TiO5 comprises the following steps:

[0112] S1. Weigh 1.8 g of CO(NH2)2 particles, add them to 60 mL of ethylene glycol solvent, stir magnetically for 30 min, and after the particles are completely dissolved, heat the solution in a water bath to a constant temperature of 30 °C.

[0113] S2, add 2.7g FeCl3·6H2O to the water bath solution obtained in step S1, stir magnetically for 30min to obtain a uniform brown solution; use a pipette to measure 3.4mL Ti(OC4H9)4, add dropwise to the above brown solution and continue stirring for 4h;

[0114] S3, pour the mixed solution in S2 into a Teflon-lined container, put it into a high-pressure reactor, place it in a constant temperature oven and hydrothermally treat it at 170°C for 7 hours, filter and wash the hydrothermal product three times with anhydrous ethanol, and dry the product in a vacuum oven at 70°C for 10 hours to obtain a catalyst precursor (Fe2TiO5 precursor);

[0115] S4. In an air atmosphere, the dried Fe2TiO5 precursor was heated to 620°C at 5°C / min, calcined at 620°C for 1.5 h, and then naturally cooled to room temperature to finally obtain brown Fe2TiO5 powder.

[0116] The solid hydrogen storage composite material provided in the present embodiment includes MgH2 and the bimetallic oxide catalyst Fe2TiO5 provided in the present embodiment, Fe2TiO5 accounts for 8wt% of the solid hydrogen storage composite material, and MgH2 accounts for 92wt% of the solid hydrogen storage composite material, wherein MgH2 is prepared by hydrogenation combustion synthesis (HCS). First, the raw magnesium powder is placed in a reaction boat in a furnace chamber for reaction. In order to avoid the presence of impurity gases such as oxygen during the reaction, the furnace chamber pressure is first evacuated to 25Pa by a vacuum pump and then filled with 0.2MPa argon gas for cleaning three times to ensure the purity of the gas in the furnace chamber, followed by filling with 2.0MPa hydrogen. Next, the Mg powder is heated from room temperature to 580°C and then kept warm for 2h at a heating rate of 10°C / min. Subsequently, the heating system is turned off and naturally cooled to 340°C and kept warm for 8h. During the reaction, the pressure can be adjusted to always keep the hydrogen pressure at 2.0MPa. Finally, the heating and hydrogen input are stopped, and the furnace chamber is naturally cooled to room temperature to obtain MgH2.

[0117] The preparation method of the solid hydrogen storage composite material provided in this embodiment includes: adding Fe2TiO5 to MgH2 prepared in this embodiment according to a mass percentage formula, and mixing by ball milling to obtain a MgH2-8 wt% Fe2TiO5 composite material; wherein the ball-to-material ratio is 30:1, the rotation speed is 400 rpm, the ball milling is 10 hours, and the work is stopped for 6 minutes every 30 minutes.

[0118] The dehydrogenation activation energy of MgH2-8 wt%Fe2TiO5 is 78.4 kJ / mol.

[0119] Example 3

[0120] The solid-state hydrogen storage composite material provided in this embodiment is the same as that in Example 1 except that the mass percentage of Fe2TiO5 is different from that in Example 1. Specifically, the solid-state hydrogen storage composite material includes MgH2 and the bimetallic oxide catalyst Fe2TiO5 provided in Example 1, Fe2TiO5 accounts for 3wt% of the solid-state hydrogen storage composite material, and MgH2 accounts for 97wt% of the solid-state hydrogen storage composite material, wherein MgH2 is prepared by the preparation method provided in Example 1.

[0121] The preparation method of the solid hydrogen storage composite material provided in this embodiment includes: adding Fe2TiO5 to MgH2 prepared in this embodiment according to a mass percentage formula, and mixing by ball milling to obtain a MgH2-3 wt.% Fe2TiO5 composite material; wherein the ball-to-material ratio is 30:1, the rotation speed is 400 rpm, the ball milling is 10 hours, and the work is stopped for 6 minutes every 30 minutes.

[0122] The dehydrogenation activation energy of MgH2-3 wt%Fe2TiO5 is 89.4 kJ / mol.

[0123] Example 4

[0124] The solid-state hydrogen storage composite material provided in this embodiment is the same as that in Example 1 except that the mass percentage of Fe2TiO5 is different from that in Example 1. Specifically, the solid-state hydrogen storage composite material includes MgH2 and the bimetallic oxide catalyst Fe2TiO5 provided in Example 1, wherein Fe2TiO5 accounts for 10wt% of the solid-state hydrogen storage composite material, and MgH2 accounts for 90wt% of the solid-state hydrogen storage composite material, wherein MgH2 is prepared by the preparation method provided in Example 1.

[0125] The preparation method of the solid hydrogen storage composite material provided in this embodiment includes: adding Fe2TiO5 to MgH2 prepared in this embodiment according to a mass percentage formula, and mixing by ball milling to obtain a MgH2-10 wt% Fe2TiO5 composite material; wherein the ball-to-material ratio is 30:1, the rotation speed is 400 rpm, the ball milling is 10 hours, and the work is stopped for 6 minutes every 30 minutes.

[0126] The dehydrogenation activation energy of MgH2-10 wt%Fe2TiO5 is 73.5 kJ / mol.

[0127] Comparative Example 1

[0128] The solid hydrogen storage composite material provided in this comparative example includes MgH2 and an iron catalyst, wherein iron accounts for 8wt% of the solid hydrogen storage composite material, and MgH2 accounts for 92wt% of the solid hydrogen storage composite material, wherein MgH2 is prepared by hydrogenation combustion synthesis (HCS). First, a raw magnesium powder is placed in a reaction boat in a furnace chamber for reaction. In order to avoid the presence of impurity gases such as oxygen during the reaction, the furnace chamber pressure is first evacuated to 25Pa by a vacuum pump and then filled with 0.2MPa argon gas for cleaning three times to ensure the purity of the gas in the furnace chamber, followed by filling with 2.0MPa hydrogen. Next, the Mg powder is heated from room temperature to 580°C and then kept warm for 2h at a heating rate of 10°C / min. Subsequently, the heating system is turned off and naturally cooled to 340°C and kept warm for 8h. During the reaction, the pressure can be adjusted to always keep the hydrogen pressure at 2.0MPa. Finally, the heating and hydrogen input are stopped, and the furnace chamber is naturally cooled to room temperature to obtain MgH2.

[0129] The preparation method of the solid hydrogen storage composite material provided in this comparative example comprises the following steps:

[0130] The Fe catalyst was added to the MgH2 prepared in this comparative example according to the mass percentage formula, and the mixture was mixed by ball milling to obtain a MgH2-8 wt% Fe composite material; wherein the ball-to-material ratio was 30:1, the rotation speed was 400 rpm, the ball milling was performed for 10 hours, and the work was stopped for 6 minutes every 30 minutes.

[0131] The dehydrogenation activation energy of MgH2-8 wt%Fe is 118.2 kJ / mol.

[0132] Comparative Example 2

[0133] The solid hydrogen storage composite material provided in this comparative example includes MgH2 and TiO2 catalyst, wherein the TiO2 catalyst accounts for 8wt% of the solid hydrogen storage composite material, and MgH2 accounts for 92wt% of the solid hydrogen storage composite material, wherein MgH2 is prepared by hydrogenation combustion synthesis (HCS). First, raw magnesium powder is placed in a reaction boat in a furnace chamber for reaction. In order to avoid the presence of impurity gases such as oxygen during the reaction, the furnace chamber pressure is first evacuated to 25Pa by a vacuum pump and then filled with 0.2MPa argon gas for cleaning three times to ensure the purity of the gas in the furnace chamber, followed by filling with 2.0MPa hydrogen. Next, the Mg powder is heated from room temperature to 580°C and then kept warm for 2h at a heating rate of 10°C / min. Subsequently, the heating system is turned off and naturally cooled to 340°C and kept warm for 8h. During the reaction, the pressure can be adjusted to always keep the hydrogen pressure at 2.0MPa. Finally, the heating and hydrogen input are stopped, and the furnace chamber is naturally cooled to room temperature to obtain MgH2.

[0134] The preparation method of the solid hydrogen storage composite material provided in this comparative example comprises the following steps:

[0135] (1) Preparation of TiO2 catalyst:

[0136] S1. Weigh 1.8 g of CO(NH2)2 particles, add them to 60 mL of ethylene glycol solvent, stir magnetically for 30 min, and after the particles are completely dissolved, heat the solution in a water bath to a constant temperature of 30 °C.

[0137] S2. Use a pipette to measure 3.4 mL of Ti(OC4H9)4 and add it dropwise into the above water bath solution and continue stirring for 4 h.

[0138] S3, pour the mixed solution in S2 into a Teflon-lined container, put it into a high-pressure reactor, place it in a constant temperature oven and perform hydrothermal treatment at 160°C for 6 hours, filter and wash the hydrothermal product three times with anhydrous ethanol, and dry the product in a vacuum oven at 60°C for 12 hours to obtain a TiO2 precursor;

[0139] S4. In an air atmosphere, the dried TiO2 precursor was heated to 600°C at 5°C / min, calcined at 600°C for 2h, and then naturally cooled to room temperature to finally obtain white TiO2 powder.

[0140] (2) Preparation of solid hydrogen storage composite material (MgH2-8 wt.% TiO2):

[0141] The TiO2 catalyst was added to the MgH2 prepared in this comparative example according to the mass percentage formula, and the mixture was mixed by ball milling to obtain a MgH2-8 wt.% TiO2 composite material; wherein the ball-to-material ratio was 30:1, the rotation speed was 400 rpm, the ball milling was performed for 10 hours, and the work was stopped for 6 minutes every 30 minutes.

[0142] The dehydrogenation activation energy of MgH2-8 wt%TiO2 is 106.7 kJ / mol.

[0143] Comparative Example 3

[0144] The solid hydrogen storage composite material provided in this comparative example includes MgH2 and Fe2O3 catalyst, wherein the Fe2O3 catalyst accounts for 8wt% of the solid hydrogen storage composite material, and MgH2 accounts for 92wt% of the solid hydrogen storage composite material, wherein MgH2 is prepared by hydrogenation combustion synthesis (HCS). First, raw magnesium powder is placed in a reaction boat in a furnace chamber for reaction. In order to avoid the presence of impurity gases such as oxygen during the reaction, the furnace chamber pressure is first evacuated to 25Pa by a vacuum pump and then filled with 0.2MPa argon gas for cleaning three times to ensure the purity of the gas in the furnace chamber, followed by filling with 2.0MPa hydrogen. Next, the Mg powder is heated from room temperature to 580°C and then kept warm for 2h at a heating rate of 10°C / min. Subsequently, the heating system is turned off and naturally cooled to 340°C and kept warm for 8h. During the reaction, the pressure can be adjusted to always keep the hydrogen pressure at 2.0MPa. Finally, the heating and hydrogen input are stopped, and the furnace chamber is naturally cooled to room temperature to obtain MgH2.

[0145] The preparation method of the solid hydrogen storage composite material provided in this comparative example comprises the following steps:

[0146] The Fe2O3 catalyst was added to the MgH2 prepared in this comparative example according to the mass percentage formula, and the mixture was mixed by ball milling to obtain a MgH2-8 wt% Fe2O3 composite material; wherein the ball-to-material ratio was 30:1, the rotation speed was 400 rpm, the ball milling was performed for 10 hours, and the work was stopped for 6 minutes every 30 minutes.

[0147] The dehydrogenation activation energy of MgH2-8 wt%Fe2O3 is 154.2 kJ / mol.

[0148] Comparative Example 4

[0149] The solid hydrogen storage composite material provided in this comparative example includes MgH2 and FeTiO3 catalyst, wherein the FeTiO3 catalyst accounts for 8wt% of the solid hydrogen storage composite material, and MgH2 accounts for 92wt% of the solid hydrogen storage composite material, wherein MgH2 is prepared by hydrogenation combustion synthesis (HCS). First, raw magnesium powder is placed in a reaction boat in a furnace chamber for reaction. In order to avoid the presence of impurity gases such as oxygen during the reaction, the furnace chamber pressure is first evacuated to 25Pa by a vacuum pump and then filled with 0.2MPa argon gas for cleaning three times to ensure the purity of the gas in the furnace chamber, followed by filling with 2.0MPa hydrogen. Next, the Mg powder is heated from room temperature to 580°C and then kept warm for 2h at a heating rate of 10°C / min. Subsequently, the heating system is turned off and naturally cooled to 340°C and kept warm for 8h. During the reaction, the pressure can be adjusted to always keep the hydrogen pressure at 2.0MPa. Finally, the heating and hydrogen input are stopped, and the furnace chamber is naturally cooled to room temperature to obtain MgH2.

[0150] The preparation method of the solid hydrogen storage composite material provided in this comparative example comprises the following steps:

[0151] The FeTiO3 catalyst was added to the MgH2 prepared in this comparative example according to the mass percentage formula, and the mixture was mixed by ball milling to obtain a MgH2-8 wt% FeTiO3 composite material; wherein the ball-to-material ratio was 30:1, the rotation speed was 400 rpm, the ball milling was performed for 10 hours, and the work was stopped for 6 minutes every 30 minutes.

[0152] The dehydrogenation activation energy of MgH2-8 wt%FeTiO3 is 92.5 kJ / mol.

[0153] Structure and properties of composite materials

[0154] The structure and performance of the MgH2-8 wt% Fe2TiO5 magnesium-based composite material prepared in Example 1 were tested and analyzed. Figure 1 -As shown in Figure 8:

[0155] Figure 1 The XRD (X-ray diffraction) pattern of the Fe2TiO5 catalyst prepared in Example 1. Figure 1 It can be observed that Fe2TiO5 has a strong and sharp diffraction peak, which represents high crystallinity and corresponds to the peak position of the standard PDF card PDF#70-2728, indicating that the catalyst has high purity and is successfully prepared.

[0156] Figure 2a is an electron microscope (SEM) image of the Fe2TiO5 catalyst prepared in Example 1. Figure 2a It can be seen that the prepared Fe2TiO5 has a "coral-like" morphology and structure, consisting of clusters with a size of about 200nm, each of which is composed of tiny nanoparticles connected to each other; Figure 2b is the particle size distribution diagram of the Fe2TiO5 catalyst prepared in Example 1, from Figure 2b It was observed that the particle size is mainly concentrated between 16-26nm. The clusters are wrapped by nanoparticles and appear "hollow" inside. In addition, the nanoparticles have clear outlines and certain pores between them, which means that the Fe2TiO5 catalyst has a large specific surface area and will be easier to disperse on MgH2 during ball milling, which is beneficial to improve the catalytic efficiency.

[0157] FIG3 is a TEM (transmission electron microscope) image of the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 under dehydrogenation ( Figure 3a ), HRTEM (high-resolution transmission electron microscopy) images and corresponding SAED (selected area electron diffraction) images ( Figure 3b , c), EDS element distribution diagram ( Figure 3d ).Depend on Figure 3a It can be seen that the specific characteristics of the microstructure of the prepared MgH2-8 wt%Fe2TiO5 in the dehydrogenated state, Figure 3b The lattice fringes and diffraction rings of and c prove that the phase of the composite material changes after dehydrogenation, and new phases of Fe, TiO2 and Fe2O3 are generated. Figure 3d It can be seen that the catalyst is evenly distributed on the surface of the Mg substrate, providing conditions for efficient catalysis.

[0158] FIG4 shows the Fe2TiO5 catalyst prepared in Example 1 of the present invention, the MgH2-8 wt% Fe2TiO5 sample in the dehydrogenated state and the Fe 2p( Figure 4a ) and Ti 2p( Figure 4b )XPS spectrum. From the figure, we can observe the valence changes of the catalyst in different states, which also proves that the catalyst undergoes obvious phase changes after dehydrogenation. The valence states of Fe and Ti correspond to the generation of new phases, which are stable in the subsequent cycle process.

[0159] Figure 5 The temperature programmed desorption (TPD) curves (5°C / min) of the MgH2-8 wt% Fe, MgH2-8 wt% TiO2, MgH2-8 wt% Fe2O3 prepared in Comparative Examples 1-3 and the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 (first three times) are compared. Figure 5It can be seen that the MgH2-8wt%Fe2TiO5 composite material begins to release hydrogen at 211.5℃, completes the dehydrogenation process at 340℃, and has a dehydrogenation capacity of 6.67wt%H2. Comparing the TPD curves of the first three times of the MgH2-8 wt%Fe2TiO5 composite material, it can be seen that the dehydrogenation performance has not changed significantly due to the generation of new phases; comparing the variable temperature dehydrogenation performance of several composite materials, it is found that the catalytic effect produced by active doping of Fe, Fe2O3 and TiO2 is far less than the catalytic effect of the phase generated in situ during the dehydrogenation process of MgH2-Fe2TiO5. Among them, the doping of an equal amount of elemental Fe shows a starting dehydrogenation temperature close to that of the MgH2-Fe2TiO5 composite material, indicating that Fe can effectively improve the starting dehydrogenation performance of the composite material, while the doping of TiO2 catalyst shows a faster dehydrogenation rate, but the doping of Fe2O3 does not bring significant improvement to MgH2.

[0160] FIG6 is the isothermal hydrogenation curve of MgH2-8 wt%Fe2TiO5 obtained in Example 1 at different temperatures, and the isothermal dehydrogenation curve of MgH2-8 wt%Fe2TiO5 at different temperatures. The initial hydrogen pressure for absorption is 3MPa, and the initial hydrogen pressure for desorption is 0.005MPa. As can be seen from FIG6, MgH2-8 wt%Fe2TiO5 can absorb 2.82wt%H2( Figure 6a ), 6.17wt% H2 was released within 1000s at 300℃( Figure 6b ) has excellent hydrogen absorption and desorption kinetics.

[0161] Figure 7a The kinetic curve of 10 hydrogen absorption and desorption cycles of the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention at 300°C is shown in FIG. Figure 7b The capacity curve of MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention after 10 cycles of hydrogen absorption and desorption at 300°C is shown in FIG. Figure 7a and Figure 7b It can be found that the capacity and kinetics of MgH2-8 wt% Fe2TiO5 have basically not changed significantly after 10 cycles of hydrogen absorption and desorption. The composite system has stable hydrogen absorption and desorption cyclicity, with an average loss of only 0.003wt% H2 per cycle. This shows that after a long period of circulation, the composite sample still has a high capacity retention rate. After 10 cycles, the hydrogen absorption capacity retention rate is 99.37%, and the dehydrogenation capacity retention rate is 99.53%.

[0162] Figure 8a The dehydrogenation curve of the MgH2-8 wt% Fe2TiO5 composite material prepared according to Example 1 of the present invention at different temperatures is fitted to the kinetic equation g(α). Figure 8bThe dehydrogenation activation energy calculation result diagram of the MgH2-8 wt% Fe2TiO5 composite material prepared in Example 1 of the present invention is shown in FIG. Figure 8a The data in combined with the Arrhenius equation calculated the corresponding dehydrogenation activation energy to be 76.72 kJ / mol, which is much lower than the 160 kJ / mol of pure MgH2, indicating the improvement of the dehydrogenation performance of the composite material.

[0163] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A bimetallic oxide catalyst, characterized in that: The bimetallic oxide catalyst includes Fe2TiO5.

2. The bimetallic oxide catalyst according to claim 1, characterized in that The Fe2TiO5 is coral-like; And / or, the Fe2TiO5 is a catalyst for magnesium-based hydrogen storage materials.

3. A method for preparing a bimetallic oxide catalyst as claimed in claim 1 or 2, characterized in that: The preparation method comprises the following steps: S1, adding urea to the solvent and stirring until dissolved, then heating to the reaction temperature and maintaining a constant temperature to obtain a constant temperature solvent; S2, adding an iron source to the constant temperature solvent obtained in step S1, stirring until the iron source is dissolved, and then adding a titanium source, stirring until the reaction is fully reacted; S3, performing hydrothermal treatment on the solution after sufficient reaction in step S2, and obtaining a catalyst precursor after post-treatment; S4, calcining the catalyst precursor obtained in step S3 to obtain the bimetallic oxide catalyst.

4. The method for preparing a bimetallic oxide catalyst according to claim 3, characterized in that: In step S1, the solvent includes ethylene glycol; and / or, in step S1, the mass ratio of the urea to the volume of the solvent is (0.02-0.04): 1 g / ml; And / or, in step S1, the heating method is a water bath or an oil bath; and / or, in step S1, the reaction temperature is 30-40°C; and / or, the iron source comprises FeCl3·6H2O; And / or, the mass ratio of the urea to the iron source is (1-3):3; And / or, the titanium source includes tetrabutyl titanate, and the molar ratio of tetrabutyl titanate to FeCl3·6H2O is 1:

1.

5. The method for preparing a bimetallic oxide catalyst according to claim 3, characterized in that: In step S2, the stirring time when the iron source is dissolved is 30-40 minutes; and / or, in step S2, adding the titanium source dropwise; And / or, in step S2, the stirring time until the reaction is fully completed is 4-5 hours; And / or, the temperature of the hydrothermal treatment is 160-180°C; And / or, the hydrothermal treatment time is 6-8h; And / or, in step S3, the post-treatment includes filtering, washing and drying the product after the hydrothermal treatment, wherein the washing solvent includes ethanol, the drying temperature is 60-80° C., and the drying time is 10-12 h; and / or, in step S4, the calcination temperature is 600-650°C; And / or, in step S4, the calcination time is 1-2h; And / or, in step S4, the calcination atmosphere is an air atmosphere.

6. A solid hydrogen storage composite material, characterized in that: The solid-state hydrogen storage composite material comprises MgH2 and a catalyst, wherein the catalyst is the catalyst according to any one of claims 1-2 or a catalyst prepared by the preparation method according to any one of claims 3-5.

7. The solid hydrogen storage composite material according to claim 6, characterized in that: The percentage of the catalyst in the solid hydrogen storage composite material is 3-10wt%; And / or, the MgH2 is prepared by hydrogenation combustion synthesis.

8. A method for preparing the solid hydrogen storage composite material according to claim 6 or 7, characterized in that: The preparation method comprises: adding the catalyst into the MgH2 according to a ratio, mixing them evenly by ball milling, and preparing the solid hydrogen storage composite material.

9. The method for preparing a solid hydrogen storage composite material according to claim 8, characterized in that: In the ball milling method, the ball milling mixing time is 8-12 hours, the ball-to-material ratio is 25-35:1, and the rotation speed is 300-500r / min.

10. Use of the solid hydrogen storage composite material according to any one of claims 6 to 7 or the solid hydrogen storage composite material prepared by the preparation method according to any one of claims 8 to 9 in a product requiring hydrogen supply.

Citation Information

Patent Citations

  • Preparation method of magnetic Fe2TiO5 photocatalytic material

    CN108479779A

  • Preparation method of metal oxide composite magnesium hydride hydrogen storage material

    CN110980635A

  • Composite catalyst for hydrogen storage material, and preparation method thereof

    CN111939893A