Catalyst for preparing 1, 2-pentanediol through furfuryl alcohol hydrogenation, preparation method of catalyst and method for preparing 1, 2-pentanediol

By using alumina and silica carriers to support copper oxide and cobalt disulfide catalysts in the hydrogenolysis reaction of furfuryl alcohol, a Cu0 and CoSx synergistic catalytic system is formed, which solves the problems of the existing catalysts' stringent reaction pressure requirements and low catalytic activity. The effect of efficient production of 1,2-pentanediol is achieved.

CN118719095AActive Publication Date: 2024-10-01WANHUA CHEM GRP CO LTD

Patent Information

Application Number
CN202410805607.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-01
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing catalyst development for hydrogenolysis of furfuryl alcohol to 1,2-pentanediol has problems such as strict reaction pressure requirements for non-noble metal catalysts, low yield of 1,2-pentanediol, and high yield of low-value tetrahydrofurfuryl alcohol. Precious metal catalysts The catalytic activity is not high, the yield of pentanediol is low, and the service life of the catalyst is short.

Method used

Catalysts using alumina and/or silica carriers to support copper oxide active components and cobalt disulfide promoters are prepared through hydrothermal reaction and roasting, and are combined with mixed gas reduction of nitrogen and hydrogen to form a Cu0 and CoSx synergistic catalytic system, optimized The metal active sites and sulfur defect sites on the catalyst surface improve catalytic activity.

Benefits of technology

It achieves cheap catalyst, mild reaction conditions, high yield of 1,2-pentanediol, simple separation process, improves the selectivity of 1,2-pentanediol, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a catalyst for preparing 1, 2-pentanediol through furfuryl alcohol hydrogenation, a preparation method of the catalyst and a method for preparing the 1, 2-pentanediol. The catalyst adopts copper oxide as an active metal and adopts a cobalt disulfide modified carrier, so that the reaction activity and selectivity of the catalyst are improved. According to the present invention, furfuryl alcohol is subjected to a reaction in the presence of the catalyst and hydrogen to generate 1, 2-pentanediol, and compared with the prior art, the method has advantages of simple reaction process, mild reaction condition, high 1, 2-pentanediol selectivity, and simple subsequent separation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a catalyst for producing 1,2-pentanediol by hydrogenating furfuryl alcohol, and a method for using the catalyst to produce 1,2-pentanediol by hydrogenating furfuryl alcohol. Background Art

[0002] 1,2-Pentanediol is a straight-chain diol containing dihydroxyl groups and relatively long-chain alkyl groups. 1,2-Pentanediol is mainly used as a key raw material for the fungicide propiconazole, and is also a raw material for polyester fibers, surfactants, and pharmaceuticals. 1,2-Pentanediol is also widely used in baby products, bath products, cosmetics, cleaning products, skin care products, and hair care products due to its excellent moisturizing and antibacterial properties.

[0003] At present, the main production process of 1,2-pentanediol is the pentene method. Pentene and peroxide are used for epoxidation, esterification and hydrolysis. This process has the disadvantages of limited sources of pentene raw materials, complex processes, production involving peroxides, high process safety risks, and a lot of corrosive wastewater, which seriously restricts the development of 1,2-pentanediol. Therefore, it is of great significance and good prospects to develop new technology routes with high production efficiency and low environmental pollution by using raw materials with a wide source of raw materials and low prices.

[0004] Furfuryl alcohol is a product obtained by hydrogenating biomass furfural. Furfural is produced by hydrolysis of common agricultural byproducts such as corn cobs. It is easy to obtain and has a significant price advantage compared to other raw materials for producing 1,2-pentanediol. The key to the catalytic hydrogenation of furfuryl alcohol lies in the development of a suitable catalyst.

[0005] Patent CN201911107004.9 discloses a method for producing 1,2-pentanediol, which is to selectively hydrogenate furfuryl alcohol under the catalytic action of a precious metal catalyst supported on a composite carrier to produce 1,2-pentanediol. This process uses a precious metal catalyst, the catalyst cost is high, and the maximum yield of 1,2-pentanediol in the product is only about 40%, while the yield of the low-value by-product tetrahydrofurfuryl alcohol reaches more than 50%.

[0006] Patent CN201310361013.7 discloses a production method for preparing 1,2-pentanediol by liquid phase selective hydrogenolysis of furfuryl alcohol. Furfuryl alcohol is selectively hydrogenated to produce 1,2-pentanediol under the catalytic action of a supported copper catalyst. The operating pressure limitation of this process is that the reaction pressure is too high, reaching 8Mpa, the reaction conditions are not mild enough, and there are disadvantages such as low furfuryl alcohol conversion rate and low 1,2-pentanediol yield.

[0007] Patent CN201320723632.6 discloses a production method for preparing 1,2-pentanediol by hydrogenolysis of furfuryl alcohol, using a loaded Pt or Ru catalyst. This process uses a precious metal catalyst, the furan ring opening activity is not high, and the maximum yield of 1,2-pentanediol in the product is only about 34%. The catalyst cost of this process is high and the yield of 1,2-pentanediol is low.

[0008] Patent CN111715264B discloses a method for preparing 1,5-pentanediol by catalytic hydrogenation of tetrahydrofurfuryl alcohol. Copper oxide is used as an active component, and one or more modifying metals selected from iron, cobalt, nickel, zinc, chromium, and vanadium are used to modify it. Titanium trisulfide is used as a co-catalyst, and the composite component is loaded on a molybdenum carbide carrier, which is applied to the preparation of 1,5-pentanediol from tetrahydrofurfuryl alcohol. This patent requires the use of non-precious metals such as iron to improve the anti-sintering performance of the copper catalyst, uses molybdenum carbide to improve the stability and activity of the copper catalyst, and uses titanium trisulfide as a co-catalyst to improve the overall electron transfer performance of the catalyst. This patent uses tetrahydrofurfuryl alcohol as a raw material and catalytically hydrogenates it to produce 1,5-pentanediol. The yield of 1,2-pentanediol is not mentioned.

[0009] Patent CN109896921B provides a method for preparing 1,5-pentanediol by catalytic hydrogenation of tetrahydrofurfuryl alcohol using a molybdenum sulfide catalyst. The catalyst carrier is cerium dioxide, the catalytic hydrogenation active metal is platinum, the platinum loading is 0.5-5wt%, and the MoS2 loading is 10-40wt%. Using this catalyst, the hydrogenation product of tetrahydrofurfuryl alcohol is mainly 1,5-pentanediol, and the by-products are n-pentanol, tetrahydropyran, 2-methyltetrahydropyran and n-pentane, and no 1,2-pentanediol is generated.

[0010] The current development of catalysts for the hydrogenolysis of furfuryl alcohol to 1,2-pentanediol has the following problems: the non-precious metal catalyst Cu has strict requirements on the reaction pressure, generally requiring a pressure of more than 8 MPa, and has disadvantages such as low yield of 1,2-pentanediol and high yield of low-value tetrahydrofurfuryl alcohol; the precious metal catalyst Pt has problems such as low catalytic activity for furan ring opening, low yield of pentanediol, and short catalyst service life. Summary of the invention

[0011] The purpose of the present invention is to provide a catalyst for preparing 1,2-pentanediol by hydrogenating furfuryl alcohol, and a process for producing 1,2-pentanediol using the catalyst, which has the advantages of cheap catalyst, mild reaction conditions, simple reaction process, high yield of 1,2-pentanediol, high yield of high-value products, etc. Compared with the existing process, the method of the present invention has a simple reaction process, mild reaction conditions, can greatly improve the selectivity of 1,2-pentanediol, and makes subsequent separation simple.

[0012] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0013] A catalyst for preparing 1,2-pentanediol by hydrogenating furfuryl alcohol comprises an aluminum oxide and / or silicon oxide carrier, a copper oxide active component loaded on the carrier, and a cobalt disulfide auxiliary agent.

[0014] The method for preparing the catalyst of the present invention comprises the following steps:

[0015] (1) adding ethylenediaminetetraacetic acid to a cobalt salt aqueous solution, and then adding sodium sulfide and sodium hydroxide to dissolve;

[0016] (2) adding a carrier to the product of step (1), performing a hydrothermal reaction, cooling, separating, washing, and drying to obtain a catalyst carrier modified with cobalt sulfide;

[0017] (3) impregnating the product of step (2) in a copper salt aqueous solution, drying, shaping, and calcining.

[0018] The cobalt salt of the present invention is selected from one or more water-soluble cobalt salts such as cobalt sulfate, cobalt nitrate, and cobalt acetate.

[0019] In step (1) of the present invention, the molar ratio of ethylenediaminetetraacetic acid to cobalt salt is 0.9-1.2:1, preferably 0.95-1.1:1.

[0020] In step (1) of the present invention, the molar ratio of sodium sulfide to cobalt salt is 2.0-2.6:1, preferably 2.0-2.2:1.

[0021] In step (1) of the present invention, the molar ratio of sodium hydroxide to cobalt salt is 0.9-1.2:1, preferably 0.95-1.1:1.

[0022] In the product of step (2) of the present invention, the mass ratio of cobalt disulfide to the carrier is 1-10%, preferably 3-5%.

[0023] In step (2) of the present invention, the temperature of the hydrothermal reaction is 120-160°C, preferably 135-145°C, and the reaction time is 10-24h, preferably 16-20h.

[0024] In step (2) of the present invention, the washing comprises washing with carbon disulfide, anhydrous ethanol and distilled water in sequence.

[0025] In step (2) of the present invention, the drying temperature is 55-65° C. and the drying time is 3-5 hours.

[0026] In step (3) of the present invention, the copper salt is selected from one or more of copper sulfate, copper nitrate, copper acetate and the like.

[0027] In step (3) of the present invention, the immersion temperature is room temperature and the time is 6 to 12 hours.

[0028] In step (3) of the present invention, the impregnated catalyst is dried in an oven at 50-120° C. for 6 to 12 hours.

[0029] In step (3) of the present invention, the calcination temperature is 500-700° C. and the calcination time is 4-12 hours.

[0030] In the catalyst, the loading amount of copper oxide is 1-30wt% of the carrier mass, preferably 10-20wt%.

[0031] The catalyst of the present invention is reduced by a mixed gas of nitrogen and hydrogen (hydrogen volume content 2-20%) at 200-450° C. for 4-10 hours and has activity.

[0032] The catalyst of the present invention has excellent catalytic performance because its surface metal active sites are Cu 0 and the synergistic catalysis of CoSx species, the metal site Cu 0 Used to adsorb and activate hydrogen, Co in CoSx can adsorb active hydrogen, and the sulfur vacancies in CoSx can anchor the hydroxyl group in furfuryl alcohol, causing it to produce oblique adsorption, promoting the hydrogenation of the C=C bond on the furan ring, and at the same time weakening and breaking the furan CO bond, thereby improving the selectivity of 1,2-pentanediol, and also producing some 1,5-pentanediol as a by-product. CoS2 is a typical cubic structure, Co 2+ Surrounded by six S - Surrounded by octahedral coordination, S - With three surrounding Co 2+ The presence of Cu promotes the reduction of CoS2. 2+ Reduced to Co atoms or Co + , thus generating sulfur defect sites suitable for catalytic reactions, which in turn is conducive to the occurrence of catalytic reactions.

[0033] In the catalyst of the present invention, when the molar ratio of CuO to CoS2 is 1-20:1, preferably 4-10:1, the defect content on the catalyst surface is better and the catalyst has a high content of Cu 0 And the ability of preferably activating hydrogen, the catalyst reaction performance is excellent.

[0034] A method for preparing 1,2-pentanediol by hydrogenating furfuryl alcohol comprises the following steps: in a hydrogenation reactor, furfuryl alcohol reacts in the presence of a catalyst and hydrogen to generate 1,2-pentanediol.

[0035] The hydrogenation reactor described in the present invention is a kettle reactor, a fixed bed reactor or a loop reactor, preferably a fixed bed reactor.

[0036] The hydrogenation of the present invention can be a direct reaction without solvent, or with a solvent, wherein the solvent is preferably an alcohol or ether with a carbon number of 1 to 4, more preferably methanol and / or THF.

[0037] The hydrogenation reaction temperature of the present invention is 100-200°C, preferably 130-150°C.

[0038] The hydrogenation reaction pressure of the present invention is 1-20 MPa, preferably 2-6 MPa.

[0039] In the hydrogenation reaction of the present invention, the furfuryl alcohol space velocity is 0.02 to 0.5 h -1 , preferably 0.06~0.2h -1 .

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] 1) Using non-precious metal copper oxide catalyst system, the cost of catalyst raw materials is low;

[0042] 2) Use cobalt disulfide as a co-catalyst to improve the reaction activity and selectivity of the catalyst;

[0043] 3) The process has a simple reaction flow, mild reaction conditions, high selectivity for 1,2-pentanediol, and a simple separation flow, which can save equipment investment and energy consumption and is suitable for industrial production. DETAILED DESCRIPTION

[0044] The present invention is described in detail below by means of specific embodiments, but the scope of the present invention is not limited to the specific embodiments.

[0045] Cobalt sulfide preparation and support modification

[0046] Example 1

[0047] Add 300ml deionized water, 11.8g cobalt nitrate hexahydrate, and 11.9g ethylenediaminetetraacetic acid to a 500ml autoclave, then add 6.5g sodium sulfide and 1.8g sodium hydroxide, and stir thoroughly until dissolved. Add 100g inert alumina powder under stirring, react at 140℃ for 16h, and after hydrothermal reaction, the generated cobalt sulfide is fully mixed with the carrier. Cool naturally to room temperature, filter, wash with carbon disulfide, anhydrous ethanol, and distilled water in turn, put into an oven, dry at 60℃ for 4h, take out and grind to make a cobalt sulfide-modified catalyst carrier-1, with a cobalt sulfide content of about 5wt% of the carrier.

[0048] Example 2

[0049] Add 300ml deionized water, 7.1g cobalt nitrate hexahydrate, and 7.1g ethylenediaminetetraacetic acid to a 500ml autoclave, then add 4.2g sodium sulfide and 1.0g sodium hydroxide, and stir thoroughly until dissolved. Add 100g inert alumina powder under stirring, react at 145℃ for 18h, and after hydrothermal reaction, the generated cobalt sulfide is fully mixed with the carrier. Cool naturally to room temperature, filter, wash with carbon disulfide, anhydrous ethanol, and distilled water in turn, put into an oven, dry at 60℃ for 4h, take out and grind to make a cobalt sulfide-modified catalyst carrier-2, with a cobalt sulfide content of about 3wt% of the carrier.

[0050] Example 3

[0051] Add 300ml deionized water, 9.5g cobalt nitrate hexahydrate, and 9.5g ethylenediaminetetraacetic acid to a 500ml autoclave, then add 5.3g sodium sulfide and 1.3g sodium hydroxide, and stir until dissolved. Add 100g inert alumina powder under stirring, react at 135℃ for 20h, and after hydrothermal reaction, the generated cobalt sulfide is fully mixed with the carrier. Cool naturally to room temperature, filter, wash with carbon disulfide, anhydrous ethanol, and distilled water in turn, put into an oven, dry at 60℃ for 4h, take out and grind to make a cobalt sulfide-modified catalyst carrier-3, with a cobalt sulfide content of about 4wt% of the carrier.

[0052] Catalyst preparation

[0053] Example 4

[0054] The catalyst was prepared by the equal amount impregnation method.

[0055] 100 g of the carrier 1 obtained in Example 1 was placed in a beaker, 47.5 g of copper nitrate was weighed and dissolved in water and then diluted to 100 ml, and the copper nitrate solution was added dropwise while being continuously stirred with a glass rod; after the addition was completed, the mixed solution was immersed at room temperature for 10 hours, and then dried in an oven at 100° C. for 6 hours, extruded into 2 mm cylindrical catalysts, and calcined at 550° C. for 10 hours to obtain catalyst 1, wherein the copper oxide loading of the catalyst was approximately 20% of the carrier, and the molar ratio of cobalt sulfide to copper oxide was approximately 1:6.5.

[0056] Example 5

[0057] 100 g of the carrier 2 obtained in Example 2 was placed in a beaker, 35.4 g of copper nitrate was weighed and dissolved in water and then diluted to 100 ml, and the copper nitrate was added dropwise while being continuously stirred with a glass rod; after the addition was completed, the mixture was immersed at room temperature for 10 hours, and then dried in an oven at 100° C. for 6 hours, extruded into 2 mm cylindrical catalysts, and calcined at 600° C. for 6 hours to obtain catalyst 2, wherein the copper oxide loading of the catalyst was approximately 15% of the carrier, and the molar ratio of cobalt sulfide to copper oxide was approximately 1:8.1.

[0058] Example 6

[0059] 100 g of the carrier 3 obtained in Example 3 was placed in a beaker, 25.6 g of copper nitrate was weighed and dissolved in water and then diluted to 100 ml, and the copper nitrate solution was added dropwise while being continuously stirred with a glass rod; after the addition was completed, the mixture was immersed at room temperature for 10 hours, and then dried in an oven at 80°C for 10 hours, extruded into 2 mm cylindrical catalysts, and calcined at 700°C for 4 hours to obtain catalyst 3, wherein the copper oxide loading of the catalyst was approximately 10% of the carrier, and the molar ratio of cobalt sulfide to copper oxide was approximately 1:4.1.

[0060] Comparative Example 1

[0061] Only 11.8 g of cobalt nitrate hexahydrate in Example 1 was replaced by 6.3 g of sodium molybdate, and other conditions remained unchanged to obtain a carrier-4 modified with molybdenum sulfide. The catalyst preparation was the same as in Example 4 to obtain a comparative catalyst 1.

[0062] Comparative Example 2

[0063] Only 11.8 g of cobalt nitrate hexahydrate in Example 1 was replaced by 10.5 g of sodium titanate, and other conditions remained unchanged to obtain titanium sulfide modified carrier-5. The catalyst preparation was the same as in Example 6 to obtain comparative catalyst 2.

[0064] Comparative Example 3

[0065] Only the carrier was changed to an alumina carrier that was not modified with cobalt sulfide, and other conditions were the same as in Example 5, to prepare a comparative catalyst 3 containing only copper oxide.

[0066] Catalyst evaluation

[0067] Example 7

[0068] 50 ml of the catalyst-1 described in Example 4 was taken and loaded into a fixed bed reactor. The catalyst was reduced with a mixture of nitrogen and hydrogen (hydrogen volume content 10%) at 260°C for 10 h before the reaction evaluation, and then cooled for reaction evaluation. The reaction hotspot temperature was 145°C, the reaction pressure was 6 MPa, and the furfuryl alcohol space velocity was 0.2 h -1The molar ratio of hydrogen to furfuryl alcohol was 40:1. A 30wt% furfuryl alcohol solution in THF was continuously pumped in. After sampling and analysis, the furfuryl alcohol conversion rate was greater than 99.9%, the selectivity for 1,2-pentanediol was 60.2%, the selectivity for 1,5-pentanediol was 20.3%, the selectivity for amyl alcohol was 8.8%, the selectivity for tetrahydrofurfuryl alcohol was 4.5%, and the selectivity for other components was 6.2% in total.

[0069] Example 8

[0070] 50 ml of the catalyst-2 described in Example 5 was taken and loaded into a fixed bed reactor. The catalyst was reduced at 300°C for 6 h using a mixture of nitrogen and hydrogen (hydrogen volume content 10%) before the reaction evaluation, and then cooled for the reaction evaluation. The reaction hotspot temperature was 140°C, the reaction pressure was 4 MPa, and the furfuryl alcohol space velocity was 0.1 h -1 The molar ratio of hydrogen to furfuryl alcohol was 40:1. A 30wt% methanol solution of furfuryl alcohol was continuously pumped in. Sampling and analysis showed that the furfuryl alcohol conversion rate was greater than 99.9%, the selectivity of 1,2-pentanediol was 58.9%, the selectivity of 1,5-pentanediol was 19.3%, the selectivity of pentanol was 9.8%, the selectivity of tetrahydrofurfuryl alcohol was 5.5%, and the selectivity of other components was 6.5% in total.

[0071] Example 9

[0072] 50 ml of the catalyst-3 described in Example 6 was taken and loaded into a fixed bed reactor. The catalyst was reduced at 300°C for 6 h using a mixture of nitrogen and hydrogen (hydrogen volume content 10%) before the reaction evaluation, and then cooled for the reaction evaluation. The reaction hotspot temperature was 135°C, the reaction pressure was 2 MPa, and the furfuryl alcohol space velocity was 0.06 h -1 The molar ratio of hydrogen to furfuryl alcohol was 40:1. A 30wt% furfuryl alcohol solution in THF was continuously pumped in. After sampling and analysis, the furfuryl alcohol conversion rate was greater than 99.8%, the selectivity for 1,2-pentanediol was 59.9%, the selectivity for 1,5-pentanediol was 19.8%, the selectivity for amyl alcohol was 10.5%, the selectivity for tetrahydrofurfuryl alcohol was 5.1%, and the selectivity for other components was 4.7% in total.

[0073] Comparative Example 4

[0074] Except that the catalyst was replaced with the catalyst described in Comparative Example 1, other operating conditions were the same as in Example 7, with a furfuryl alcohol conversion rate of 99.5%, a 1,2-pentanediol selectivity of 32.1%, a 1,5-pentanediol selectivity of 10.4%, a tetrahydrofurfuryl alcohol selectivity of 40.5%, a pentanol selectivity of 4.5%, and a total selectivity of other components of 12.5%.

[0075] Comparative Example 5

[0076] Except that the catalyst was replaced with the catalyst described in Comparative Example 2, other operating conditions were the same as in Example 9, with a furfuryl alcohol conversion rate of 99.6%, a 1,2-pentanediol selectivity of 28.6%, a 1,5-pentanediol selectivity of 11.3%, a tetrahydrofurfuryl alcohol selectivity of 33.5%, a pentanol selectivity of 7.5%, and a total selectivity of other components of 19.1%.

[0077] Comparative Example 6

[0078] Except that the catalyst was replaced with the catalyst described in Comparative Example 3, other operating conditions were the same as in Example 8, with a furfuryl alcohol conversion rate of 99.7%, a 1,2-pentanediol selectivity of 33.6%, a 1,5-pentanediol selectivity of 12.5%, a tetrahydrofurfuryl alcohol selectivity of 29.5%, a pentanol selectivity of 12.4%, and a total selectivity of other components of 12.0%.

[0079] Comparative Example 7

[0080] Except that the catalyst was replaced with the carrier described in Example 1 and no active metal component was added, other operating conditions were the same as in Example 7, with a furfuryl alcohol conversion rate of 7.9%, a 1,2-pentanediol selectivity of 8.9%, a 1,5-pentanediol selectivity of 4.8%, a tetrahydrofurfuryl alcohol selectivity of 74.5%, a pentanol selectivity of 2.5%, and a total selectivity of other components of 9.3%.

[0081] It can be seen from the above examples that the present invention is simple to operate, can greatly improve the yield of the target product 1,2-pentanediol and high-value 1,5-pentanediol, and simplifies the separation process.

Claims

1. A catalyst for preparing 1,2-pentanediol by hydrogenating furfuryl alcohol, comprising an aluminum oxide and / or silicon oxide carrier, a copper oxide active component supported on the carrier, and a cobalt disulfide additive.

2. The catalyst according to claim 1, characterized in that The loading amount of copper oxide is 1-30wt% of the carrier mass, preferably 10-20wt%.

3. The catalyst according to claim 1, characterized in that The molar ratio of copper oxide to cobalt disulfide is 1-20:1, preferably 4-10:

1.

4. A method for preparing the catalyst according to claim 1, comprising the following steps: (1) adding ethylenediaminetetraacetic acid to a cobalt salt aqueous solution, and then adding sodium sulfide and sodium hydroxide to dissolve; (2) adding a carrier to the product of step (1), performing a hydrothermal reaction, cooling, separating, washing, and drying to obtain a catalyst carrier modified with cobalt sulfide; (3) impregnating the product of step (2) in a copper salt aqueous solution, drying, shaping, and calcining.

5. The method according to claim 4, characterized in that The cobalt salt is selected from one or more of cobalt sulfate, cobalt nitrate and cobalt acetate.

6. The method according to claim 4, characterized in that In step (1), the molar ratio of EDTA to cobalt salt is 0.9-1.2:1, preferably 0.95-1.1:1; the molar ratio of sodium sulfide to cobalt salt is 2.0-2.6:1, preferably 2.0-2.2:

1.

7. The method according to claim 4, characterized in that In step (2), the temperature of the hydrothermal reaction is 120-160° C., preferably 135-145° C., and the reaction time is 10-24 h, preferably 16-20 h.

8. The method according to claim 4, characterized in that The copper salt is selected from one or more of copper sulfate, copper nitrate and copper acetate.

9. The method according to claim 4, characterized in that In the step (3), the calcination temperature is 500 to 700° C. and the calcination time is 4 to 12 hours.

10. A method for preparing 1,2-pentanediol by hydrogenating furfuryl alcohol, comprising the following steps: In a hydrogenation reactor, furfuryl alcohol is reacted in the presence of the catalyst of claim 1 and hydrogen to produce 1,2-pentanediol; preferably, the hydrogenation reaction temperature is 100-200°C, preferably 130-150°C; the hydrogenation reaction pressure is 1-20Mpa, preferably 2-6Mpa; the furfuryl alcohol space velocity is 0.02-0.5h -1 , preferably 0.06~0.2h -1 .

Citation Information

Patent Citations

  • Method for preparing 1,2-pentanediol by furfuryl alcohol liquid phase selectivity and hydrogenolysis

    CN104370702A

  • Method for preparing 1,5-pentanediol by using catalyst containing molybdenum disulfide for catalytic hydrogenation of tetrahydrofurfuryl alcohol

    CN109896921A

  • Catalyst for synthesizing 1, 2-pentanediol and preparation method thereof

    CN116459831A

  • catalytic liquid phase hydrogenation process which can be used for the purification of light hydrocarbons

    FR1237708A

Cited By

  • Method for synthesizing 1, 2-pentanediol through furfuryl alcohol hydrogenation

    CN122685500A