Porous spherical water-resistant sulfur-resistant low-temperature SCR (Selective Catalytic Reduction) denitration catalyst and preparation method thereof

By adopting the design of porous spherical structure and hydrophobic layer in the low-temperature SCR catalyst, the problem of activity decrease of the low-temperature catalyst in the environment of water and sulfur oxides is solved, and efficient NOx removal and water and sulfur resistance are achieved, which is suitable for industry Flue gas treatment.

CN118719110APending Publication Date: 2024-10-01HEFEI UNIV OF TECH +1

Patent Information

Application Number
CN202410735120.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing low-temperature SCR catalysts have low NOx denitration efficiency in flue gas and are intolerant to water and sulfur oxides, resulting in reduced catalyst activity and difficulty in effectively reducing NOx emissions under low-temperature conditions.

Method used

A water-resistant and sulfur-resistant low-temperature SCR denitration catalyst with a porous spherical structure is used. The anatase TiO2 is ball milled and combined with active components, metal additives and hydrophobic materials to form nano-porous spherical particles, which are then subjected to segmented calcination and Chemical vapor deposition builds a hydrophobic layer to enhance the water resistance and denitrification activity of the catalyst.

Benefits of technology

It significantly improves the NOx removal rate and water and sulfur resistance of the catalyst, reduces production costs, is suitable for industrial applications, and maintains efficient denitrification performance under low temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719110A_ABST
    Figure CN118719110A_ABST
Patent Text Reader

Abstract

The invention discloses a porous spherical water-resistant sulfur-resistant low-temperature SCR denitration catalyst and a preparation method thereof. The SCR denitration catalyst for treating water-containing and sulfur-containing flue gas structurally comprises a catalyst carrier and active components adsorbed on the surface of the carrier and outside a hydrophobic material cavity, and nitrogen-containing groups are grafted to carboxyl or lactone groups on anatase titanium dioxide treated by oxalic acid to promote oxidation of NO, so that a denitration reaction is carried out towards a rapid SCR reaction; the surface of each hydrophobic cavity is composed of hydroxyl, the catalyst carrier body comprises an anatase titanium dioxide substrate, active components and nitrogen-containing functional groups are uniformly distributed on the carrier, and the hydrophobic cavities are arranged in order to form a hydrophobic layer. The catalyst provided by the invention can effectively improve the denitration efficiency of the industrial flue gas denitration catalyst, is easy to operate, and can overcome the defects that the existing catalyst has low denitration efficiency at low temperature, and the catalyst is inactivated when containing water vapor and sulfur dioxide, so that the denitration efficiency is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of vanadium-based denitration catalyst preparation, and in particular relates to a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst and a preparation method thereof. Background Art

[0002] Flue gas from boilers, combustion of fossil fuels and exhaust gas from cars all contain nitrogen oxides. As one of the sources of air pollution, nitrogen oxides not only cause photochemical smog, acid rain, PM2.5 and greenhouse effect, but also NO x The NO in it can combine with hemoglobin in the human body to produce hypoxia, causing lung and respiratory diseases, seriously endangering human safety and the natural environment.

[0003] Currently, the selective catalytic reduction of NO by ammonia x (NH3-SCR) Vanadium supported on titania catalysts are widely used in medium and high temperature NO x The main principle of emission reduction is that the reducing agent (usually ammonia) reduces NO in the flue gas under the action of a catalyst. x Converted into nitrogen and water. For flue gas with low temperature (usually below 300°C), directly heating the flue gas consumes huge energy. Although manganese-based catalysts have good catalytic activity at low temperatures, when encountering SO2 and H2O in the flue gas, the catalysts easily form sulfates, causing the catalyst activity to drop quickly or even completely deactivate.

[0004] In order to overcome this problem, the study found that although the catalytic activity of vanadium-based catalysts at low temperatures is not as high as that at medium and high temperatures, they have certain water and sulfur resistance, so it is necessary to modify the catalyst to improve the low-temperature denitrification activity while further strengthening the catalyst's resistance to SO2 and H2O. According to the survey of relevant literature, many researchers have improved the low-temperature activity and sulfur resistance of V / TiO2 catalysts by metal (Ce, Nb, Fe, etc.) doping and acidification (solid acid acidification, acidification in a sulfur-containing atmosphere). Then, a hydrophobic core-shell structure is constructed on the outside of the catalyst (such as SiO2@Mn catalyst and FeMn@Si-C catalyst). Although the catalyst with a core-shell structure has a certain water resistance, the process of preparing the core-shell structure is not only quite complicated, but the prepared core-shell structure may also affect the entry of the reaction molecules and affect the denitrification activity, and the core-shell structure is not resistant to high temperatures. Therefore, in the later stage, a nitrogen-doped hierarchical porous vanadium-based catalyst was constructed by adding a special nitrogen-containing group (pyridine-type nitrogen group) through transition metal composite doping modification and calcination in a nitrogen atmosphere to improve the catalyst's adsorption and oxidation of NO, so that the standard SCR catalytic reaction can be transformed into a fast SCR, thereby improving the denitration efficiency of the low-temperature vanadium-based catalyst. Then, a hydrophobic channel and a hydrophobic layer were constructed by wet ball milling and chemical vapor deposition to improve water resistance. The hydrophobic layer is not only simple to prepare but also can significantly improve the denitration efficiency of its low-temperature sulfur-resistant and water-resistant catalyst. Summary of the invention

[0005] In order to overcome the problem that the existing catalyst mainly undergoes standard SCR reaction during the denitration reaction, and a very small amount of rapid SCR reaction occurs, resulting in low denitration efficiency and poor water and sulfur resistance. The present invention provides a porous spherical water and sulfur resistant low-temperature SCR denitration catalyst. The catalyst prepared by the method can effectively improve the denitration efficiency and water and sulfur resistance of the catalyst, and is easy to operate.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst comprises the following steps:

[0008] S1, adding a certain amount of oxalic acid to anatase TiO2 and dissolving it in an ethanol solution for ball milling to obtain nanoporous spherical particles of TiO2;

[0009] S2, adding active component precursor, metal additive, phosphate, transition metal oxide, nitrogen-containing compound to a certain concentration of organic acid solution, stirring and immersing until completely dissolved, and then adding nano-porous spherical particle TiO2 carrier to obtain a porous spherical SCR catalyst precursor;

[0010] S3. Drying, calcining, and wet ball-milling or vapor-depositing the porous spherical SCR catalyst precursor to add a hydrophobic layer to obtain the porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst.

[0011] Preferably, the porous spherical structure includes, from the inside to the outside, small particles of porous TiO2, active components scattered in the carrier pores and in the middle layer on the surface, and nitrogen-containing groups grafted to the carboxyl or lactone groups on the surface of titanium dioxide, and the outermost layer is a mixture of hydrophobic materials and active components. The active components are evenly distributed on the hydrophilic layer outside the hydrophobic cavity of the barreled structure to occupy the sites, so that water molecules in the flue gas directly enter the hydrophobic cavity for elimination, thereby reducing the inactivation of the active components due to contact with water.

[0012] Preferably, the ball milling treatment specifically includes: adding a certain amount of oxalic acid to anatase TiO2, dissolving the solution in ethanol, and putting the solution into a ball mill, and controlling the rotation speed to 300-600 rpm.

[0013] Preferably, the active component precursor is ammonium metavanadate or ammonium vanadate;

[0014] The metal additives include molybdate and ammonium phosphomolybdate;

[0015] The phosphate is ammonium phosphate or diammonium hydrogen phosphate;

[0016] The transition metal oxide is one of nano Co3O4, nano La2O3 and nano ZrO2.

[0017] Preferably, in S3, the catalyst precursor is dried at a temperature of 90-120° C. and for a drying time of 3-6 h.

[0018] Preferably, the nitrogen-containing compound comprises melamine or pyridine.

[0019] Preferably, the organic acid is oxalic acid, which is used as a co-solvent for the active component precursor, and has a mass concentration of 1-3 wt%.

[0020] Preferably, during the stirring and immersion in S2, the heating temperature is 60-120°C, the rotation speed is 400-800 rpm, and the immersion time is 1-4 hours.

[0021] Preferably, the catalyst precursor calcination conditions in S3 are:

[0022] The dried porous spherical SCR catalyst precursor is placed in a tubular furnace and calcined by passing nitrogen;

[0023] Stage I is to heat up to 120-250°C at 5-20°C / min and keep warm for 1h; Stage I is to remove adsorbed water and decompose excess organic acid at room temperature to form the pre-calcination stage;

[0024] Stage II is to heat up to 350-450℃ at 5-20℃ / min and keep warm for 3h; Stage II is the temperature stage for decomposition, calcination and enhancement of active components and pore forming;

[0025] Stage III is the stage of slowly decreasing to room temperature at a rate of 5 to 20°C / min. Stage III is the stage of gradually decreasing to room temperature.

[0026] Preferably, the hydrophobic material is one or more of β-cyclodextrin (barreled structure, hydrophobic wrapping of active components in the cavity, hydrophilic rapid transport of water molecules outside the cavity), polydimethylsiloxane (PDMS) (defective hydrophobic PDMS film is enriched near the active site of the vanadium-based catalyst) and polydivinylbenzene (PDVB) (the hydrophobic layer of the membrane structure is enriched near the active site).

[0027] A porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst, the SCR denitration catalyst comprises the following raw materials in percentage by mass: 1-10wt% of the active component precursor, 5-20wt% of the metal additive, 1-5wt% of the phosphate, 1-8wt% of the transition metal oxide, 1-5wt% of the nitrogen-containing compound, 1-10wt% of the hydrophobic material, and the rest is a nano-spherical particle TiO2 carrier.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. The present invention adopts a method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst, which has a higher denitration efficiency in the flue gas denitration process. Compared with the catalyst prepared by high-temperature calcination in the prior art, under the same state, NO x The removal rate is significantly improved.

[0030] 2. The staged calcination method of the present invention sets stage II as the active component decomposition calcination stage, which is carried out with a slow temperature rise, and can form a microporous reaction structure on the catalyst surface and in the pores, so that the active components, metal additive precursors and nitrogen-containing compounds are slowly and evenly decomposed at high temperature to form V2O5, MoO3 and nitrogen-containing groups, etc., which are dispersed in the carrier pores, increasing the active sites and the surface nitrogen content. The heat is kept for 3 hours to ensure that the catalytic active sites and the nitrogen content are evenly distributed, thereby forming a highly dispersed structure of the catalytic active sites and the nitrogen content in the carrier pores, maintaining the excellent catalytic activity and stability of the catalyst.

[0031] 3. The main body of the SCR denitration catalyst prepared by the present invention includes an anatase titanium dioxide substrate, and the active components and nitrogen-containing functional groups are evenly distributed on the carrier. The active components are evenly distributed inside or outside the carrier pores and outside the hydrophobic material barrel structure. The nitrogen-containing groups are grafted onto the carboxyl or lactone groups to promote the oxidation of NO and make the denitration reaction proceed to a fast SCR reaction; due to the orderly arrangement of the hydrophobic cavities, a hydrophobic layer is formed. The catalyst of the present invention can effectively improve the denitration efficiency of the industrial flue gas denitration catalyst, is easy to operate, and can overcome the shortcomings of the existing catalysts in the production process, such as poor denitration efficiency at low temperatures, deactivation of the catalyst due to the presence of water vapor and sulfur dioxide, thereby reducing the denitration efficiency. It has a high denitration efficiency, high yield, low cost, and is easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 This is a comparative activity evaluation diagram of the porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst prepared in Example 1 of the present invention and the sulfur resistance of Comparative Example 3.

[0034] Figure 2 It is a comparison chart of the denitration and water resistance performance of the porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst prepared in Example 1 of the present invention and that of Comparative Example 3.

[0035] Figure 3 This is a graph showing the long-term water and sulfur resistance activity evaluation of the porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst prepared in Example 1 of the present invention.

[0036] Figure 4 It is a schematic diagram of the synthesis structure of the porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst of the present invention. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Preparation Example

[0039] 50 g of anatase TiO2 was added to 10 g of oxalic acid, dissolved in 200 ml of ethanol solution, and put into a ball mill with the rotation speed controlled at 500 rpm to obtain a nano-spherical particle TiO2 carrier.

[0040] Example 1

[0041] A method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst comprises the following steps:

[0042] Step 1: Dissolve 0.83g oxalic acid in 50ml deionized water, heat and stir until completely dissolved, add 0.39g ammonium metavanadate and stir until the solution turns dark blue, then add 0.74g ammonium molybdate and 0.108g diammonium hydrogen phosphate, add 0.1g nano Co3O4 and 0.2g melamine after dissolution, and finally add 9.05g of the TiO2 carrier in the preparation example, stir and soak for 2h.

[0043] Step 2: Place the uniform solution obtained in step 1 in a 108° C. oven and dry for 4 hours to obtain an impregnated dried embryo.

[0044] Step 3: The impregnation liquid dried embryo obtained in step 2 is crushed and put into a tubular furnace for roasting. Stage I is to heat up to 250°C at 5°C / min and keep warm for 1h; stage II is to heat up to 450°C at 10°C / min and keep warm for 3h; stage III is to cool down to room temperature at 10°C / min.

[0045] Step 4: The obtained catalyst was crushed and added with 1.0 g of β-cyclodextrin into an ethanol solution and placed in a ball mill at a speed of 300 rpm for ball milling. Finally, it was placed in an oven at 80°C for drying. The dried catalyst was crushed into 40-60 mesh to obtain catalyst 1 (TiO2@VMoCoN@CD) for activity evaluation.

[0046] Example 2

[0047] A method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst comprises the following steps:

[0048] Step 1: Dissolve 0.83g oxalic acid in 50ml deionized water, heat and stir until completely dissolved, add 0.39g ammonium metavanadate and stir until the solution turns dark blue, then add 0.74g ammonium molybdate and 0.108g diammonium hydrogen phosphate, add 0.1g nano La2O3 and 0.2g melamine after dissolution, and finally add 9.05g of the TiO2 carrier in the preparation example, stir and soak for 2h.

[0049] Step 2: Place the uniform solution obtained in step 1 in a 108°C oven and dry for 4 hours.

[0050] Step 3: The impregnation liquid dried embryo obtained in step 2 is crushed and put into a tubular furnace for roasting. Stage I is heated to 120°C at 6°C / min and kept warm for 1 hour; stage II is heated to 350°C at 10°C / min and kept warm for 3 hours; stage III is cooled to room temperature at 10°C / min.

[0051] Step 4: The obtained catalyst was crushed and added with 1.0 g of β-cyclodextrin into an ethanol solution and placed in a ball mill at 300 rpm for ball milling. Finally, it was placed in an oven at 80°C for drying. The dried catalyst was crushed into 40-60 mesh to obtain catalyst 2 (TiO2@VMoLaN@CD) for activity evaluation.

[0052] Example 3

[0053] A method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst comprises the following steps:

[0054] Step 1: Dissolve 0.83g oxalic acid in 50ml deionized water, heat and stir until completely dissolved, add 0.39g ammonium metavanadate and stir until the solution turns dark blue, then add 0.74g ammonium molybdate and 0.108g diammonium hydrogen phosphate, add 0.1g nano ZrO2 and 0.2g melamine after dissolution, and finally add 9.05g of the TiO2 carrier in the preparation example, stir and soak for 2h.

[0055] Step 2: Place the uniform solution obtained in step 1 in an oven at 108°C and dry for 5 hours.

[0056] Step 3: The impregnation liquid dried embryo obtained in step 2 is crushed and put into a tubular furnace for roasting. In stage I, the temperature is increased to 200°C at 8°C / min and kept warm for 1 hour; in stage II, the temperature is increased to 400°C at 8°C / min and kept warm for 3 hours; in stage III, the temperature is reduced to room temperature at 20°C / min.

[0057] Step 4: The obtained catalyst was crushed and added with 1.0 g of β-cyclodextrin into an ethanol solution and placed in a ball mill at 300 rpm for ball milling. Finally, it was placed in an oven at 80°C for drying. The dried catalyst was crushed into 40-60 mesh to obtain catalyst 3 (TiO2@VMoZrN@CD) for activity evaluation.

[0058] Example 4

[0059] A method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst comprises the following steps:

[0060] Step 1: Dissolve 0.83g oxalic acid in 50ml deionized water, heat and stir until completely dissolved, add 0.39g ammonium metavanadate and stir until the solution turns dark blue, then add 0.74g ammonium molybdate and 0.108g diammonium hydrogen phosphate, add 0.1g nano ZrO2 after dissolution, and finally add 9.05g TiO2 carrier in the preparation example, stir and soak for 2h.

[0061] Step 2: Place the uniform solution obtained in step 1 in an oven at 108°C and dry for 5 hours.

[0062] Step 3: The impregnation liquid dried embryo obtained in step 2 is crushed and put into a tubular furnace for roasting. Stage I is to heat up to 250°C at 10°C / min and keep warm for 1 hour; stage II is to heat up to 400°C at 20°C / min and keep warm for 3 hours; stage III is to cool down to room temperature at 20°C / min.

[0063] Step 4: The obtained catalyst was crushed and put into a solution containing 0.2g pyridine and 50ml deionized water for immersion for 1h and dried. Then, it was added into an ethanol solution with 1.0g β-cyclodextrin and put into a ball mill at a speed of 300rpm for ball milling. Finally, it was put into an oven at 80℃ for drying. The dried catalyst was crushed into 40-60 mesh to obtain catalyst 4 (TiO2@VMoZr-N@CD) for activity evaluation.

[0064] Example 5

[0065] A method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst comprises the following steps:

[0066] Step 1: Dissolve 0.83g oxalic acid in 50ml deionized water, heat and stir until completely dissolved, add 0.39g ammonium metavanadate and stir until the solution turns dark blue, then add 0.74g ammonium molybdate and 0.108g diammonium hydrogen phosphate, add 0.1g nano ZrO2 and 0.2g melamine after dissolution, and finally add 9.05g of the TiO2 carrier in the preparation example, stir and soak for 2h.

[0067] Step 2: Place the uniform solution obtained in step 1 in an oven at 108°C and dry for 5 hours.

[0068] Step 3: The impregnation liquid dried embryo obtained in step 2 is crushed and put into a tubular furnace for roasting. Stage I is to heat up to 250°C at 10°C / min and keep warm for 1 hour; stage II is to heat up to 450°C at 20°C / min and keep warm for 3 hours; stage III is to cool down to room temperature at 15°C / min.

[0069] Step 4: The obtained catalyst and 1.0 g of polydivinylbenzene (PDVB) were added to a certain amount of ethanol solution for wet ball milling. After drying, the mixture was ground and crushed with a glass mortar and sieved to 50 mesh to obtain catalyst 5 (TiO2@VMoZrN@VB) for activity evaluation.

[0070] Example 6

[0071] A method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst comprises the following steps:

[0072] Step 1: Dissolve 0.83g oxalic acid in 50ml deionized water, heat and stir until completely dissolved, add 0.39g ammonium metavanadate and stir until the solution turns dark blue, then add 0.74g ammonium molybdate and 0.108g diammonium hydrogen phosphate, add 0.1g nano ZrO2 and 0.2g melamine after dissolution, and finally add 9.05g of the TiO2 carrier in the preparation example, stir and soak for 2h.

[0073] Step 2: Place the uniform solution obtained in step 1 in a 108°C oven and dry for 6 hours.

[0074] Step 3: The impregnation liquid dried embryo obtained in step 2 is crushed and put into a tubular furnace for roasting. Stage I is to heat up to 200°C at 10°C / min and keep warm for 1 hour; stage II is to heat up to 400°C at 15°C / min and keep warm for 3 hours; stage III is to cool down to room temperature at 10°C / min.

[0075] Step 4: Grind the obtained catalyst with a glass mortar and crush it, then sieve it to 50 mesh. Apply 1.0 g of a thin layer of hydrophobic material polydimethylsiloxane (PDMS) on the surface of the 50-mesh catalyst particles by chemical vapor deposition to obtain catalyst 6 (TiO2@VMoZrN@MS) for activity evaluation.

[0076] Comparative Example 1

[0077] The method of Example 3 is implemented, except that the process of step 4 is:

[0078] The calcined catalyst was sieved to 60 mesh with a sieve, and the β-cyclodextrin hydrophobic layer was not sprayed on the catalyst surface, thereby obtaining catalyst 1 (TiO2@VMoZrN), which was directly used for activity evaluation.

[0079] Comparative Example 2

[0080] The method of Example 4 is implemented, except that the process of step 4 is:

[0081] Other reagents were added normally without adding pyridine solution to obtain catalyst 2 (TiO2@VMoZr@CD).

[0082] Comparative Example 3

[0083] The method of Example 1 was followed, except that in step 1, other reagents were added normally without adding melamine solution; and in step 4, the catalyst obtained by calcination was sieved with a 60-mesh sieve without adding a β-cyclodextrin hydrophobic layer, to obtain catalyst 3 (TiO2@VMoCo) for activity evaluation.

[0084] The catalyst activity test method is:

[0085] The porous spherical water-resistant and sulfur-resistant low-temperature SCR denitrification catalyst was tested for activity in an activity evaluation device composed of a fixed bed device and an online flue gas analysis device. The denitrification activity of Examples 1 to 6 was evaluated under the conditions of 80 to 300°C, 500 ppm nitrogen oxides, 100 ppm sulfur dioxide and 10% water content.

[0086] The test results are shown in Table 1.

[0087] Table 1 NO of porous spherical water-resistant and sulfur-resistant catalysts of Examples 1-6 and Comparative Examples 1-3 x Conversion rate and water resistance

[0088]

[0089] As can be seen from Table 1, the catalyst with water resistance can accelerate the transport of water molecules or keep away from water molecules because its surface provides hydrophobic channels or hydrophobic layers, thereby showing higher water resistance and sulfur resistance; the nitrogen-containing groups grafted onto the carboxyl or lactone groups improve the adsorption and oxidation capacity of NO, thereby improving the low-temperature denitration efficiency of the catalyst. In summary, the method of the present invention not only has a high ability to resist deactivation for flue gas containing water vapor and sulfur dioxide, but also the porous spherical sulfur-resistant catalyst has a high denitration efficiency at low temperatures.

[0090] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst, characterized in that: The following steps are involved: S1, ball milling anatase TiO2 to obtain nano-spherical particles of TiO2; S2, adding a certain concentration of organic acid solution, stirring and immersing until completely dissolved, and then adding a nano porous spherical particle TiO2 carrier to obtain a porous spherical SCR catalyst carrier; S3. The porous spherical SCR catalyst carrier is immersed in a solution to which an active component precursor, a metal additive, a phosphate, a transition metal oxide and a nitrogen-containing group are added, and then dried and calcined. The calcined catalyst is added to an ethanol solution containing a hydrophobic material, ball-milled, and dried to obtain a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst.

2. The method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst according to claim 1, characterized in that: The porous spherical structure includes, from inside to outside, a small-particle porous TiO2 carrier as the center, active components distributed on the surface or in the pores of the carrier, and nitrogen-containing groups grafted onto the carboxyl or lactone groups on the titanium dioxide treated with oxalic acid, while the outermost layer is composed of a hydrophobic material arrangement.

3. The method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst according to claim 1, characterized in that: The nitrogen-containing compound includes melamine or pyridine.

4. The method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst according to claim 2, characterized in that: The hydrophobic material is one or more of β-cyclodextrin, polydimethylsiloxane and polydivinylbenzene.

5. The method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst according to claim 1, characterized in that: The ball milling treatment specifically includes: adding oxalic acid to anatase TiO2 dissolved in ethanol solution and putting it into a ball mill to make TiO2 present a more porous structure, and after the acidification treatment, the carboxyl and lactone groups on the surface of TiO2 can better combine with nitrogen-containing groups, controlling the rotation speed to 300-600rpm, and finally drying to obtain small-particle porous TiO2.

6. The method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst according to claim 1, characterized in that: The active component precursor is ammonium metavanadate or ammonium vanadate; The metal additive includes molybdate such as ammonium molybdate and ammonium phosphomolybdate; The phosphate is ammonium phosphate or diammonium hydrogen phosphate; The transition metal oxide is one of nano Co3O4, nano La2O3 and nano ZrO2.

7. The method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst according to claim 1, characterized in that: The catalyst precursor in S3 is dried at a temperature of 90-120° C. and for a drying time of 3-6 hours.

8. The method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst according to claim 1, characterized in that: The organic acid is oxalic acid, and the mass concentration is 1-3wt%.

9. The method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst according to claim 1, characterized in that: During the stirring and immersion in S2, the heating temperature is 60-120°C, the rotation speed is 400-800 rpm, and the immersion time is 1-4 hours.

10. The method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst according to claim 1, characterized in that: The catalyst precursor calcination conditions in S3 are: The dried porous spherical SCR catalyst precursor is placed in a tubular furnace and calcined by passing nitrogen; Stage I: heating at 5-20℃ / min to 120-250℃, keeping warm for 1h; Stage II: heating to 350-450℃ at 5-20℃ / min and keeping warm for 3h; Stage III is to slowly cool down to room temperature at a rate of 5-20°C / min.

11. An SCR denitration catalyst prepared by the method for preparing a porous spherical water-resistant and sulfur-resistant low-temperature SCR denitration catalyst according to any one of claims 1 to 10, characterized in that: The SCR denitration catalyst includes the following raw materials in percentage by mass: 1-10wt% of the active component precursor, 5-20wt% of the metal additive, 1-5wt% of the phosphate, 1-8wt% of the transition metal oxide, 1-5wt% of the nitrogen-containing compound, 1-10wt% of the hydrophobic material, and the rest is a nanoporous spherical particle TiO2 carrier.

Citation Information

Patent Citations

  • Wide-temperature sulfur-resistant water-resistant vanadium-titanium denitration catalyst and preparation method thereof

    CN112121831A

  • Low-temperature denitration catalyst as well as preparation method and application thereof

    CN114682247A

  • Modified carbon-based catalyst for NH3-SCR denitration and preparation method thereof

    CN117463386A

  • Preparation method for sulfur poisoning-resistant electric denitration catalyst

    WO2024022073A1