Application of diamino ether amine in flotation desiliconization of new magnetite

By using bis-aminoetheramine as a collector for nascent magnetite, the problem of insufficient performance of the nascent magnetite flotation collector in the existing technology is solved, and efficient iron ore separation and high-grade iron concentrate are achieved. Mine production.

CN118719332APending Publication Date: 2024-10-01KUNMING UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411077892.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing magnetite flotation collectors have problems with poor low-temperature resistance, poor foam fluidity, and low selectivity in newborn magnetite, and cannot effectively adapt to changes in the physical and chemical properties of roasted hematite after magnetization. .

Method used

Bisaminoetheramine (PPDA) is used as the reverse flotation desilicon collector of newborn magnetite. It improves low-temperature solubility and foam performance through its ether structure and branched chain structure, and improves the interaction with the new magnetite through hydrogen bonding and electrostatic attraction. Separation effect of silicon-containing gangue.

Benefits of technology

It improves the flotation effect of newborn magnetite, enhances the iron grade, simplifies the flotation process, achieves high selectivity and high recovery rate, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004982876920000021
    Figure BDA0004982876920000021
  • Figure FDA0004982876910000011
    Figure FDA0004982876910000011
Patent Text Reader

Abstract

The invention discloses application of diamino ether amine in flotation desilicication of newly-generated magnetite, and belongs to the technical field of iron ore flotation separation. The diamino ether amine has an ether group structure and a branched chain structure, the ether group structure and the branched chain structure can effectively improve the low-temperature solubility and the foam performance and enhance the steric effect, on one hand, the diamino group can increase the action capacity with the silicon-containing gangue, and the diamino group and the silicon-containing gangue form hydrogen-bond interaction and electrostatic attraction simultaneously; and on the other hand, the specific space structure of the diamino group can increase the electrostatic repulsive force and steric effect of the reagent and the surface of the new magnetite, and when the diamino group is used for flotation separation of the new magnetite (magnetic concentrate obtained after magnetic separation of roasted hematite) and silicon-containing gangue minerals, the flotation effect can be effectively improved. The natural magnetite and the new magnetite obtained after hematite roasting have obvious difference in property, the collecting agent is specially researched and developed according to the characteristics of the new magnetite, and the collecting agent is high in selectivity, short in flotation process and easy to industrialize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron ore flotation separation, in particular to application of bisaminoetheramine in flotation desiliconization of newborn magnetite. Background Art

[0002] Iron ore resources are the raw materials of the steel industry and play a vital role in the national economy. Hematite is the most common iron ore resource and often coexists with silicate minerals. For difficult-to-select hematite, studies in recent years have found that it can be converted into new magnetite through multi-stage suspended magnetization roasting, and then the new magnetite is separated by magnetic separation. However, since strong magnetic magnetite will produce strong interaction forces after magnetization, and fine-grained minerals are also very sensitive to electrostatic forces, van der Waals forces and other forces, some quartz will still enter the magnetic concentrate. Therefore, in order to obtain high-grade iron concentrate, it is necessary to further separate quartz and other silicon-containing gangue minerals mixed in the magnetic concentrate. Flotation is one of the most efficient methods for separating silicon-containing gangue minerals in magnetic concentrate.

[0003] At present, the main magnetite flotation collector is amine collector, but traditional amine collectors have problems such as poor low temperature resistance, poor foam fluidity, and low selectivity. In addition, the physical and chemical properties of the newly generated magnetite after magnetization and roasting of hematite are quite different from those of natural magnetite. The existing magnetite collectors are not suitable for the newly generated magnetite system. Therefore, it is very necessary to develop a flotation desiliconization collector suitable for newly generated magnetite. Summary of the invention

[0004] The purpose of the present invention is to provide an application of bisaminoetheramine in the flotation desiliconization of new magnetite to solve the problems existing in the above-mentioned prior art.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention is: an application of a bisaminoetheramine (PPDA for short) in the flotation desiliconization of new magnetite, wherein the bisaminoetheramine is used as a collector for reverse flotation desiliconization of new magnetite; the structural formula of the bisaminoetheramine is

[0007]

[0008] Furthermore, the newly formed magnetite is a magnetic concentrate obtained by magnetic separation of roasted hematite.

[0009] That is, the preparation method of the new magnetite is: roasting hematite and magnetically separating it to obtain the new magnetite.

[0010] Furthermore, the Fe grade of the new magnetite is 55-65%, and the SiO 2 The grade is less than 20%.

[0011] Furthermore, the SiO 2 The grade is preferably 5-10%.

[0012] Furthermore, in the new magnetite, the components with a particle size less than 0.074 mm account for 70-90% by mass.

[0013] Furthermore, the flotation desiliconization step of the newly formed magnetite includes: mixing bisaminoetheramine with water to obtain a collector solution; mixing the newly formed magnetite with water to obtain a pulp; adjusting the pH of the pulp to 3-12, and then adding the collector solution to perform flotation scraping.

[0014] Furthermore, the mass percentage concentration of the collector solution is 0.01-0.5%.

[0015] Furthermore, the mass percentage concentration of the slurry is 20-30%.

[0016] Furthermore, the collector solution is added to the ore pulp in an amount of 50-120 g / t.

[0017] Furthermore, the specific operation of adjusting the pH value of the ore pulp to 3-12 is: adding 0.2-3% by mass concentration of HCl solution or NaOH solution to the ore pulp to adjust the pH value of the ore pulp to 3-12, and the slurry adjustment time is 2-3 minutes.

[0018] Furthermore, the collector solution is added for 3-5 minutes.

[0019] Furthermore, the flotation scraping time is 3-5 minutes.

[0020] Furthermore, after the flotation frothing is completed, a flotation foam product and an in-tank product are obtained.

[0021] Furthermore, the flotation is specifically reverse flotation, and after the flotation froth is scraped to obtain the flotation foam product and the product in the tank, the flotation product in the tank is also subjected to a post-processing step, wherein the post-processing step is as follows: drying the product in the tank to obtain an iron concentrate; the iron concentrate has an Fe grade of 64-68%, and SiO 2 The grade is less than 2%; the recovery rate of the iron ore concentrate is 85-93%.

[0022] Furthermore, the flotation temperature is 10-25°C.

[0023] The present invention aims at the shortcomings of existing magnetite collectors and the technical vacancy of new magnetite flotation reagents, and provides an application of a bisamino ether amine collector PPDA in the flotation desiliconization of new magnetite. The ether structure and branched structure of the bisamino ether amine can effectively improve low-temperature solubility, foam performance and enhance steric effect. On the one hand, the bisamino group can increase the ability to interact with silicon-containing gangue, and simultaneously form hydrogen bonding and electrostatic attraction with the silicon-containing gangue. On the other hand, the specific spatial structure of the bisamino group can increase the electrostatic repulsion and steric effect of the reagent and the surface of the new magnetite. It is used for the flotation separation of new magnetite (magnetic separation concentrate of hematite after magnetic separation after roasting) and silicon-containing gangue minerals, which can effectively improve the flotation effect. In addition, the collector has the characteristics of simple synthesis, wide source of raw materials, good foam performance, high solubility at low temperature, good selectivity, etc., and can effectively improve the iron grade in the magnetic separation concentrate of hematite after roasting, which is of great significance for the production of high-quality iron concentrate.

[0024] The present invention discloses the following technical effects:

[0025] (1) The newly generated magnetite after roasting natural magnetite and hematite has differences in properties such as surface roughness, charging characteristics, and contact angle. The present invention specifically targets the characteristics of newly generated magnetite and uses a bisaminoetheramine with a special structure as a collector for flotation desiliconization of newly generated magnetite. The collector has high selectivity, a short flotation process, and is easy to industrialize.

[0026] (2) Compared with the current magnetite collector, the collector of the present invention has the advantages of good low temperature resistance, small dosage, strong selectivity, and easy synthesis. DETAILED DESCRIPTION

[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0028] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0032] The "room temperature" referred to in the following examples and comparative examples specifically refers to 20-25°C.

[0033] Example 1

[0034] (1) Selection of new magnetite: The new magnetite (magnetic concentrate) used in this example is obtained by roasting and magnetic separation of hematite, and its chemical composition is as follows: TFe content is 58wt%, SiO 2 The content is 7.45wt%, Al 2 O 3 The content is 7.15wt%, the CaO content is 0.20wt%, and the MgO content is 0.26wt%; by mass, the components with a particle size of less than 0.074mm in the new magnetite account for 80%.

[0035] (2) Preparation of bisaminoetheramine collector solution:

[0036] The bisaminoetheramine prepared in Example 1 was mixed with water at a mass ratio of 0.5:100 at room temperature, and stirred at a speed of 1000 r / min for 5 min to obtain a collector solution with a mass percentage concentration of 0.5%.

[0037] (3) Pulping and flotation

[0038] The newly formed magnetite is mixed with water to prepare a slurry with a mass percentage concentration of 20%, and then a 1% HCl solution with a mass percentage concentration is added to the slurry to adjust the pH of the slurry to 5, and the slurry adjustment time is 3 minutes. Then, the above-mentioned collector solution is added to the slurry in an amount of 100g / t, and the adding time is 3 minutes. Then, the aeration is turned on, and flotation and foaming are carried out at 10°C for 5 minutes to obtain the flotation tank product and the foam product.

[0039] (4) Post-processing of the product in the tank: The product in the tank obtained in step (3) is dried to obtain a Fe grade of 64%, SiO 2 The iron ore concentrate has a grade of 1.5% and an iron ore recovery rate of 90%.

[0040] Example 2

[0041] (1) Selection of new magnetite: The new magnetite (magnetic concentrate) used in this example is obtained by roasting and magnetic separation of hematite, and its chemical composition is as follows: TFe content is 62wt%, SiO 2 The content is 6.05wt%, Al 2 O 3 The content is 5.11wt%, the CaO content is 0.4wt%, and the MgO content is 0.6wt%; by mass, the components with a particle size of less than 0.074mm in the new magnetite account for 85%.

[0042] (2) Preparation of bisaminoetheramine collector solution:

[0043] The bisaminoetheramine prepared in Example 1 was mixed with water at a mass ratio of 0.5:100 at room temperature, and stirred at a speed of 1000 r / min for 5 min to obtain a collector solution with a mass percentage concentration of 0.5%.

[0044] (3) Pulping and flotation

[0045] The newly formed magnetite is mixed with water to prepare a slurry with a mass percentage concentration of 25%, and then a HCl solution with a mass percentage concentration of 0.2% is added to the slurry to adjust the pH of the slurry to 4.5, and the slurry adjustment time is 4 minutes. Then, the above-mentioned collector solution is added to the slurry in an amount of 60g / t, and the adding time is 5 minutes. Then, the aeration is turned on, and flotation and foaming are carried out at 10°C for 4 minutes to obtain the flotation tank product and the foam product.

[0046] (4) Post-processing of the product in the tank: The product in the tank obtained in step (3) is dried to obtain a Fe grade of 67%, SiO 2 The iron concentrate has a grade of 0.5% and an iron concentrate recovery rate of 89%.

[0047] Example 3

[0048] (1) Selection of new magnetite: The new magnetite (magnetic concentrate) used in this example is obtained by roasting and magnetic separation of hematite, and its chemical composition is as follows: TFe content is 62wt%, SiO 2 The content is 6.05wt%, Al 2 O 3 The content is 5.11wt%, the CaO content is 0.4wt%, and the MgO content is 0.6wt%; by mass, the components with a particle size of less than 0.074mm in the new magnetite account for 85%.

[0049] (2) Preparation of bisaminoetheramine collector solution:

[0050] The bisaminoetheramine prepared in Example 1 was mixed with water at a mass ratio of 0.5:100 at room temperature, and stirred at a speed of 1000 r / min for 5 min to obtain a collector solution with a mass percentage concentration of 0.5%.

[0051] (3) Pulping and flotation

[0052] The newly formed magnetite is mixed with water to prepare a slurry with a mass percentage concentration of 25%, and then a NaOH solution with a mass percentage concentration of 0.2% is added to the slurry to adjust the pH of the slurry to 11, and the slurry adjustment time is 4 minutes. Then, the above-mentioned collector solution is added to the slurry in an amount of 80g / t, and the adding time is 5 minutes. Then, the aeration is turned on, and flotation and foaming are carried out at 10°C for 4 minutes to obtain the flotation tank product and the foam product.

[0053] (4) Post-processing of the product in the tank: The product in the tank obtained in step (3) is dried to obtain a Fe grade of 66%, SiO 2 The iron concentrate has a grade of 0.7% and an iron concentrate recovery rate of 86%.

[0054] Comparative Example 1

[0055] The same as Example 2, except that the collector used in step (1) is replaced by another ether amine collector (structural formula: ), the difference between the etheramine collector and the bisaminoetheramine of the present invention is that there are three methylene groups between the ether group and the amino group. After flotation and post-treatment of the product in the tank, the comparative example obtained Fe grade of 62.4%, SiO 2 The grade of the iron concentrate is 5.97%, and the recovery rate of the iron concentrate is 90%. Although the collector used in this comparative example is also a branched etheramine agent, it cannot separate the gangue and the newly formed magnetite.

[0056] Comparative Example 2

[0057] Same as Example 3, except that the new magnetite is replaced by a magnetic concentrate obtained by magnetic separation of natural magnetite, and its TFe content is 62wt%, SiO 2 The content is 7wt%, and the components with a particle size of less than 0.074mm account for 85% by mass. After flotation and post-treatment of the product in the tank, the Fe grade of this comparative example is 63%, SiO 2 The grade of the iron concentrate is 5.8%, and the recovery rate of the iron concentrate is 55%. By comparing this comparative example with Example 3, it can be found that the physical and chemical properties of natural magnetite and roasted new magnetite are different, and the indicators of natural magnetite and roasted new magnetite flotation with the same flotation reagent are quite different.

[0058] Comparative Example 3

[0059] The same as Example 2, except that the collector used in step (1) is replaced by common amine collector dodecylamine. 2 The iron concentrate has a grade of 5.6% and an iron concentrate recovery rate of 65%.

[0060] Comparative Example 4

[0061] Same as Example 2, except that the collector was replaced with α-octane ether amino-dodecanoic acid, and the minerals were magnetic concentrates (with a TFe content of 28wt%, SiO 2 content of 48wt%) and magnetic separation concentrate after direct magnetic separation of natural magnetite (with a TFe content of 62wt%, SiO 2 The content of the two minerals is 7wt%), and the components with a mass particle size of less than 0.074mm account for 85%. Two groups of flotation experiments were carried out under the same flotation conditions as in Example 2. The results showed that the hematite and the gangue could not be separated. The Fe grade of the obtained iron concentrate was 29%, the recovery rate was 40%, and the SiO 2 The grade is 47%; the natural magnetite has a certain separation effect from the gangue, and the iron concentrate obtained has an Fe grade of 65% and a recovery rate of 84%. 2 The grade is 1.5%. It can be seen that the same collector has different flotation effects on different types of iron ore.

[0062] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. Application of bisaminoetheramine in flotation desiliconization of new magnetite, characterized in that: The bisaminoetheramine is used as a collector for flotation desiliconization of new magnetite; the structural formula of the bisaminoetheramine is 2. The use according to claim 1, characterized in that The new magnetite is a magnetic concentrate obtained by magnetic separation of roasted hematite.

3. The use according to claim 1, characterized in that The Fe grade of the new magnetite is 55-65%, and the SiO2 grade is less than 20%.

4. The use according to claim 1, characterized in that The components with a particle size of less than 0.074 mm account for 70-90% by mass of the new magnetite.

5. The use according to claim 1, characterized in that The steps of flotation desiliconization of the newly formed magnetite include: mixing bisaminoetheramine with water to obtain a collector solution; mixing the newly formed magnetite with water to obtain a pulp; adjusting the pH of the pulp to 3-12, then adding the collector solution, and performing flotation frothing.

6. The use according to claim 5, characterized in that The mass percentage concentration of the collector solution is 0.01-0.5%.

7. The use according to claim 5, characterized in that The mass percentage concentration of the ore pulp is 20-30%.

8. The use according to claim 5, characterized in that The collector solution is added in an amount of 50-120 g / t in the ore pulp.

Citation Information

Patent Citations

  • Method for separating roasted iron core and jade in floatation mode through cation combined collecting agents

    CN102698876A

  • Reverse-flotation desiliconizing method for hematite ore

    CN105435968A