Manufacturing process of high-strength TC4 titanium alloy plate

By using sponge titanium, aluminum vanadium master alloy and titanium dioxide powder ingredients, vacuum plasma welding box and vacuum consumable electric arc furnace melting in the manufacturing process of TC4 titanium alloy, combined with step heating and multi-pass rolling process, the problem is solved In the existing technology, the problems of low rolling efficiency and high cost of TC4 titanium alloy have been achieved, and the production of plates with high strength and good uniformity has been achieved to meet the performance requirements of aerospace and other fields.

CN118719799APending Publication Date: 2024-10-01SHENYANG TONGXING IND

Patent Information

Application Number
CN202410845611.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing rolling process of TC4 titanium alloy requires high temperature strength, resulting in high rolling capacity and narrow temperature window, resulting in low rolling efficiency and high cost, making it difficult to meet the requirements for uniform performance and grain grade in aerospace and other fields.

Method used

Using sponge titanium, aluminum vanadium master alloy, aluminum particles and high purity titanium dioxide powder ingredients, through vacuum plasma welding box electrode assembly welding and vacuum consumable electric arc furnace melting, multiple melting and lathe peeling, combined with step heating and Multi-pass rolling process, controlled rolling temperature and annealing treatment to ensure the uniformity and strength of the finished plate.

Benefits of technology

It achieves the uniform structure and excellent performance of high-strength TC4 titanium alloy sheets, simplifies the rolling process, improves efficiency, reduces production costs, meets national standard requirements, and significantly improves the punching strength.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a manufacturing process of a high-strength TC4 titanium alloy plate, the manufacturing process of the high-strength TC4 titanium alloy plate is formulated, the pass deformation amount is reasonably arranged, the total rolling deformation amount can exceed 85%, the TC4 titanium alloy plate with excellent structure performance can be obtained, and the titanium alloy plate rolled through the manufacturing process is good in structure uniformity, good in surface quality and high in strength. The titanium alloy plate can meet the requirements of the national standard and has good stamping resistance, the rolling technology is simplified, the rolling efficiency is improved, and the production cost is remarkably reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium alloy plates, and specifically relates to a manufacturing process of a high-strength TC4 titanium alloy plate. Background Art

[0002] TC4 titanium alloy is a titanium alloy with the grade of TC4. Its material composition is Ti-6Al-4V, which belongs to α+β type titanium alloy. TC4 titanium alloy has excellent corrosion resistance, low density, high specific strength, good toughness and weldability, and is widely used in aerospace, petrochemical, shipbuilding, automobile, medicine and other fields. At present, titanium alloys used in aerospace and military fields require uniform transverse and longitudinal performance organization, grain grade ≥9 or homogeneous titanium alloy.

[0003] Due to the high temperature strength of TC4 titanium alloy, high requirements are placed on the rolling capacity of the rolling mill. At the same time, the temperature window is very narrow when two-phase rolling is used. Therefore, a multi-pass rolling process is usually adopted. This can reduce the deformation amount of a single pass and reduce the load on the rolling mill. Using fewer total rolling passes per pass can reduce the rolling time and ensure the final rolling temperature.

[0004] Therefore, a manufacturing process of high-strength TC4 titanium alloy plate is proposed, which can reduce the rolling process and improve the rolling efficiency. Summary of the invention

[0005] The object of the present invention is to provide a manufacturing process for a high-strength TC4 titanium alloy plate to solve the problems raised in the above background technology.

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a manufacturing process of a high-strength TC4 titanium alloy plate, which comprises the following steps: using sponge titanium, aluminum-vanadium master alloy, aluminum particles and titanium dioxide powder with a purity greater than 99.5% to prepare and press electrodes, using a vacuum plasma welding box to perform electrode assembly welding, using a vacuum consumable arc furnace to perform smelting, the smelting times are not less than 2 times, after the last smelting, cutting off the ingot riser and lathe peeling to obtain an ingot, the components and mass fractions of the obtained ingot are: Al: 6.5%, V: 4.1%, Fe: 0.15%, C: 0.02%, O: 0.165%, N: 0.02%, H: 0.005%, the remainder is Ti, and the electrode pressing is completed on a hydraulic press according to the batching list, and the electrode is smelted into a uniform component after three vacuum consumable or plasma cooling furnaces, and the specific implementation is as follows:

[0007] S1. Preheat the ingot to a temperature of 980°C to 1050°C in the soaking section;

[0008] S2, rolling the heated ingot;

[0009] S3, annealing the rolled plate, air-cooling it after it is taken out of the furnace, and obtaining a finished plate.

[0010] The rolling temperature is 850°C to 1000°C, and the final rolling temperature is greater than or equal to 800°C;

[0011] The first three rolling passes adopt large reduction, the deformation of a single pass meets 20-30%, the deformation of the middle pass is controlled at 15-20%, and the deformation of the last pass is controlled at 5-10%.

[0012] The finished plate has a thickness of 15 to 30 mm.

[0013] The temperature of the finished product annealing in S3 is 620°C to 700°C, and the annealing time is 2-5h.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] By formulating the manufacturing process of high-strength TC4 titanium alloy plates and reasonably arranging the deformation amount of each pass, the total rolling deformation can exceed 85%, and the TC4 titanium alloy plates with excellent organizational properties can be obtained. The titanium alloy plates rolled by the present invention have good organizational uniformity and good surface quality, and can meet the requirements of national standards. The titanium alloy plates in the present invention have good stamping strength resistance, and the rolling process is simplified, the rolling efficiency is improved, and the production cost is significantly reduced. DETAILED DESCRIPTION

[0016] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] The invention provides a manufacturing process of a high-strength TC4 titanium alloy plate. Sponge titanium, aluminum-vanadium master alloy, aluminum particles and titanium dioxide powder with a purity greater than 99.5% are used for batching and pressing electrodes, and then a vacuum plasma welding box is used for electrode assembly welding. A vacuum consumable arc furnace is used for smelting, and the smelting times are not less than 2 times. After the last smelting, the riser of the ingot is cut off and the ingot is peeled on a lathe to obtain an ingot. The components and mass fractions of the obtained ingot are: Al: 6.5%, V: 4.1%, Fe: 0.15%, C: 0.02%, O: 0.165%, N: 0.02%, H: 0.005%, and the remainder is Ti. The thickness of the slab is 120-150 mm.

[0018] A manufacturing process of a high-strength TC4 titanium alloy plate comprises the following steps: S1, heating a slab by a walking beam heating furnace, wherein the heating temperature and the holding time are controlled by a stepping cycle, and the stepping cycle is obtained by calculating the length of each heating section and the stepping length of the heating furnace, so as to meet the following step heating conditions: a preheating section is less than 800°C and is kept warm for 60 to 90 minutes, a heating section is 880 to 930°C and is kept warm for 60 to 90 minutes, and a soaking section is 980 to 1050°C and is kept warm for 60 to 90 minutes;

[0019] After the soaking time is completed, the soaking temperature is increased to 1000-1020°C, and the soaking temperature is continued for 30-60 minutes, followed by hot rolling.

[0020] S2, rolling the heated ingot, with the starting rolling temperature being ≥950°C and the final rolling temperature being greater than 800°C;

[0021] S3, annealing the rolled plate, air-cooling it after it is taken out of the furnace, and obtaining a finished plate.

[0022] S4. The annealing temperature of the finished product is 620℃~700℃, and the annealing time is 2-5h

[0023] Among them, in the manufacturing process of the above-mentioned TC4 titanium alloy plate, the first three passes of rolling described in S2 use a large reduction, the deformation of a single pass meets 20-30%, the deformation of the middle pass is controlled at 15-20%, and the deformation of the last pass is controlled at 5-10%.

[0024] The finished plate has a thickness of 15 to 30 mm.

[0025] Embodiment 1

[0026] S1. Use a walking beam heating furnace to heat the TC4 slab with a thickness of 120 mm. The preheating section is kept at 800°C for 90 min, the heating section is kept at 930°C for 60 min, and the soaking section is kept at 980°C for 90 min.

[0027] S2, after the soaking section is kept warm for 90 minutes, the temperature of the soaking section is increased to 1050°C, and the temperature is kept warm for 30 minutes, and then the steel is taken out of the furnace and rolled;

[0028] S3, the starting rolling temperature is 965℃, the deformations of the first three passes are 22%, 30% and 28% respectively, the deformations of the middle passes are controlled at 15-20%, the deformation of the last pass is 8%, and the final rolling temperature is 880℃; after 9 rolling passes, the thickness of the finished plate is 17.4mm and the total deformation is 85.5%.

[0029] S4: The rolled slab is subjected to annealing heat treatment at a temperature of 650°C and a holding time of 4 hours, and then taken out of the furnace and air-cooled.

[0030] S5 samples were taken for mechanical property testing, with tensile strength of 868.6MPa, yield strength of 846.7MPa, and elongation of 14.5%

[0031] The obtained structure is a basketweave structure with an average grain size of 13 μm.

[0032] Embodiment 2

[0033] S1. Use a walking beam heating furnace to heat the TC4 slab with a thickness of 130 mm. The preheating section is kept at 800°C for 90 min, the heating section is kept at 930°C for 60 min, and the soaking section is kept at 980°C for 90 min.

[0034] S2, after the soaking section is kept warm for 90 minutes, the temperature of the soaking section is increased to 1050°C, and the temperature is kept warm for 30 minutes, and then the steel is taken out of the furnace and rolled;

[0035] S3, the starting rolling temperature is 974℃, the deformations of the first three passes are 21%, 29% and 26% respectively, the deformations of the middle passes are controlled at 15-20%, the deformation of the last pass is 7%, and the final rolling temperature is 820℃; after 9 rolling passes, the thickness of the finished plate is 19.5mm and the total deformation is 85%.

[0036] S4: The rolled slab is subjected to annealing heat treatment at a temperature of 950°C and a holding time of 4 hours, and then taken out of the furnace and air-cooled.

[0037] S5 samples were taken for mechanical property testing, with tensile strength of 908.6MPa, yield strength of 876.2MPa, and elongation of 14.5%

[0038] The obtained structure is a basket structure with an average grain size of 23 μm.

[0039] Embodiment 3

[0040] S1. Use a walking beam heating furnace to heat the TC4 slab with a thickness of 140 mm. The preheating section is kept at 800°C for 90 min, the heating section is kept at 930°C for 60 min, and the soaking section is kept at 980°C for 90 min.

[0041] S2, after the soaking section is kept warm for 90 minutes, the temperature of the soaking section is increased to 1050°C, and the temperature is kept warm for 30 minutes, and then the steel is taken out of the furnace and rolled;

[0042] S3, the starting rolling temperature is 992℃, the deformations of the first three passes are 23%, 28% and 28% respectively, the deformations of the middle passes are controlled at 15-20%, the deformation of the last pass is 6%, and the final rolling temperature is 850℃; after 9 rolling passes, the thickness of the finished plate is 24.3mm and the total deformation is 82.6%.

[0043] S4: The rolled slab is subjected to annealing heat treatment at a temperature of 950°C and a holding time of 4 hours, and then taken out of the furnace and air-cooled.

[0044] S5 samples were taken for mechanical property testing, with tensile strength of 930.1MPa, yield strength of 845.6MPa, and elongation of 14.5%

[0045] The obtained structure is a basket structure with an average grain size of 34 μm.

[0046] Embodiment 4

[0047] S1. Use a walking beam heating furnace to heat the TC4 slab with a thickness of 150 mm. The preheating section is kept at 800°C for 90 min, the heating section is kept at 930°C for 60 min, and the soaking section is kept at 980°C for 90 min.

[0048] S2, after the soaking section is kept warm for 90 minutes, the temperature of the soaking section is increased to 1050°C, and the temperature is kept warm for 30 minutes, and then the steel is taken out of the furnace and rolled;

[0049] S3, the starting rolling temperature is 978℃, the deformations of the first three passes are 23%, 29% and 29% respectively, the deformations of the middle passes are controlled at 15-20%, the deformation of the last pass is 8%, and the final rolling temperature is 820℃; after 9 rolling passes, the thickness of the finished plate is 26.5mm and the total deformation is 82.3%.

[0050] S4: The rolled slab is subjected to annealing heat treatment at a temperature of 950°C and a holding time of 4 hours, and then taken out of the furnace and air-cooled.

[0051] S5 samples were taken for mechanical property testing, with tensile strength of 926.6MPa, yield strength of 836.7MPa, and elongation of 13.3%

[0052] The obtained structure is a basket structure with an average grain size of 38 μm.

[0053] The TC4 titanium alloy medium and thick plates obtained by rolling in the embodiment have excellent mechanical properties and can meet the requirements of the national standard GB / T-3621-2007 on mechanical properties, with a tensile strength of ≥895MPa, a yield strength of ≥830, and an elongation of ≥8.

[0054] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A manufacturing process for high-strength TC4 titanium alloy sheet, characterized in that: After using sponge titanium, aluminum-vanadium master alloy, aluminum particles and titanium dioxide powder with a purity greater than 99.5% to prepare and press electrodes, a vacuum plasma welding box is used for electrode assembly welding, and a vacuum consumable arc furnace is used for smelting, and the number of smelting times is not less than 2 times. After the last smelting, the ingot riser is cut off and the lathe is peeled to obtain an ingot. The components and mass fractions of the obtained ingot are: Al: 6.5%, V: 4.1%, Fe: 0.15%, C: 0.02%, O: 0.165%, N: 0.02%, H: 0.005%, and the remainder is Ti. The electrode is pressed on a hydraulic press according to the ingredient list. The electrode passes through three vacuum consumable or plasma cooling furnaces to melt a component with uniform composition. The specific steps are as follows: S1. Preheat the ingot to a temperature of 980°C to 1050°C in the soaking section; S2, rolling the heated ingot; S3, annealing the rolled plate, air-cooling it after it is taken out of the furnace, and obtaining a finished plate.

2. The manufacturing process of the high-strength TC4 titanium alloy sheet according to claim 1 is characterized in that: The hot rolling temperature is such that the temperature reaches 1030-1080°C in the soaking section, and the final rolling temperature is greater than or equal to 800°C.

3. The manufacturing process of the high-strength TC4 titanium alloy sheet according to claim 2 is characterized in that: The first three hot rolling passes adopt large reduction, the deformation of a single pass meets 20-30%, the deformation of the middle pass is controlled at 15-20%, and the deformation of the last pass is controlled at 5-10%.

4. The manufacturing process of the high-strength TC4 titanium alloy sheet according to claim 3 is characterized in that: The finished plate has a thickness of 15 to 30 mm.

5. The manufacturing process of the high-strength TC4 titanium alloy sheet according to claim 1, characterized in that: The temperature of the finished product annealing in S3 is 620°C to 700°C, and the annealing time is 2-5h.

Citation Information

Patent Citations

  • Preparation method of TC4 titanium alloy plate material for 3C products

    CN107475653A

  • Single fire rolling method of TC4 titanium alloy moderate-thickness plate

    CN107952794A

  • Method for producing TC4 titanium alloy wide and thick plate by adopting direct rolling process

    CN111036703A

  • Method for preparing TC4 titanium alloy sputtering target at low cost

    CN111441020A

  • Method for producing TC4ELI titanium alloy medium plate with high yield and low cost

    CN118045863A

Cited By

  • Method for inhibiting rolling edge cracks of titanium alloy

    CN122057784A