Laser modular repairing method based on standardized modified surface defects
Through standardized repair and modular laser automatic repair database, the problem of low automation of mold repair technology is solved, efficient, high-quality, and stable mold repair is achieved, which is suitable for the repair of various high value-added surface defects.
Patent Information
- Application Number
- CN202410836795.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
AI Technical Summary
The existing mold repair technology has a low degree of automation, the repair quality depends on the operator's level and experience, and there is a lack of standardized repair process, resulting in inconsistent repair quality and difficulty in large-scale management.
Using a laser modular repair method based on standardized repair, by classifying and grading mold surface damage, performing standardized machining repair preprocessing, formulating a standardized laser repair process, and establishing a modular laser automatic repair database to achieve different damages Automated repair of damage type and level.
It improves the efficiency and quality consistency of mold repair, reduces dependence on experience, and achieves efficient, high-quality, and stable mold repair, which is suitable for the repair of various high value-added surface defects.
Smart Images

Figure CN118720169A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical fields of laser additive manufacturing, laser cladding, etc., and specifically relates to a laser modular repair method for surface defects based on standardized shaping. Background Art
[0002] Moulds are very important tools in industrial production, and they generally have common problems such as high manufacturing costs and long manufacturing cycles. For moulds with surface damage (such as "missing blocks", "corrosion", "wear", etc.), if they are directly scrapped, the service life of the mould will be short and the manufacturing cost will remain high. If high value-added moulds are repaired multiple times and continued to be used to extend their service life, the manufacturing cost of the mould can be further reduced.
[0003] Take the hot working die H13 steel as an example. During the service process, it is repeatedly in contact with the processed material in a high temperature state. The failure forms are mainly thermal fatigue failure, wear failure and corrosion failure. These failure sources usually appear on the surface of the parts. The commonly used mold repair technologies now mainly include arc surfacing, plasma surfacing, thermal spraying, laser cladding, etc. The essence of these technologies is to use a high-energy density heat source to melt the selected alloy material and then cool and solidify it in the area to be repaired, so as to achieve the purpose of covering the original defects. After the repair, the cladding area generally needs to undergo post-processing processes such as grinding and shaping to make the mold reach the specified use size and accuracy. From the perspective of the metallurgical quality after repair, due to the relatively large heat input of arc surfacing and plasma surfacing, the cooling rate in the molten pool formed after the material is melted is lower than that of laser cladding, and the grain size and thermal stress are relatively large. Of course, the processing efficiency of laser cladding is lower than that of arc and plasma, which belongs to "slow work and fine work". The alloy materials used in the above-mentioned traditional maintenance methods are basically determined, and the repair process is also relatively mature. The main problems are:
[0004] (1) The damage forms of molds are complex and diverse, and the failure positions are uncertain. Therefore, it is difficult for existing repair methods to form a unified processing flow, which is not conducive to standardized management during large-scale repair.
[0005] (2) Both pre-processing (machining and shaping pre-processing) and maintenance process (arc welding, plasma welding) are still mainly done manually. Although the laser cladding technology based on multi-axis robots can automatically carry out repairs, it is necessary to manually focus, plan the cladding path, and set the process parameters before starting the repair. Each time the repair position is changed, the above steps need to be repeated. In general, the degree of automation of mold repair technology is low, and the quality of repair depends largely on the level and experience of the operator. The consistency and reliability of the repair quality are relatively low;
[0006] (3) There is a lack of standardized repair process flow. The essence is that the damage shape and size are diverse, which results in relatively poor quality consistency in the repair area.
[0007] To sum up, it is necessary to make further innovations on existing technologies. Summary of the invention
[0008] In view of the technical problems existing in the above-mentioned background technology, the present invention proposes a modular laser repair method for mold steel surface defects based on standardized profiling. The method has a reasonable concept, which implements standardized profiling from pre-processing, and then implements standardized laser cladding process, develops serialized and standardized processes, forms a stable process database, reduces the dependence of product quality on experience, and realizes efficient, high-quality and stable mold repair.
[0009] In order to solve the above technical problems, the present invention provides a laser modular repair method based on standardized shaping of surface defects, which first classifies and grades the surface damage morphology of the mold to be repaired to sort out regular and quantifiable damage types and damage repair levels; then, according to the damage type and damage repair level, the mold to be repaired is subjected to standardized machining shaping pretreatment; then, the mold to be repaired after the standardized machining shaping pretreatment is clamped and positioned; then, a standardized laser repair process is formulated for surface defects of each damage type and damage repair level in the mold to be repaired after standardized shaping; and then a modular laser automatic repair database with standardized shaping is established to realize the automatic repair of surface defects of different damage types and damage repair levels in the mold to be repaired.
[0010] The laser modular repair method based on standardized shaping of surface defects, wherein the process of classifying and grading the damage morphology of the mold to be repaired is:
[0011] The damage defects occurring on the outer surface of the mold are classified into plane damage, edge damage and corner damage according to the location and shape of the damage, and the actual damage shape and size of the mold are counted;
[0012] For planar damage, the following three levels of damage repair are defined:
[0013] Grade I injury: d<d0,
[0014] Grade II injury: d0≤d<d1,
[0015] Grade III injury: d1≤d<d2,
[0016] Among them, d is the maximum characteristic size of the damaged area, d0, d1, and d2 are the maximum sizes of the plane damage states of level I, level II, and level III respectively obtained based on the probability statistics method; if d is greater than d2, it can be identified as level III damage first, and the damage size of the defective area can be remeasured after repair to determine the repair level, and the cycle is repeated until the repair area is completely coated;
[0017] The following three levels of damage repair are defined for both edge damage and corner damage:
[0018] Grade I injury: d<l0,
[0019] Grade II injury: l0≤d<l1,
[0020] Grade III injury: l1≤d<l2,
[0021] l0, l1, and l2 are the maximum dimensions under level I, level II, and level III edge damage and corner damage conditions respectively obtained based on the probability statistics method. For the case where d is greater than l2, it can be first identified as level III damage, and then the damage level of the defective area can be re-judged after repair. This cycle is repeated until the repaired area is completely coated.
[0022] The laser modular repair method for standardized surface defect repair, wherein: the rule is: each type of damage has a maximum characteristic size, and the probability distribution characteristics of each defect can be obtained by statistically analyzing the damage characteristic size; the quantification is: statistically analyzing the damage characteristic size of the damaged mold, classifying each damage size according to the probability of occurrence, and grading the damage based on the statistical results.
[0023] The laser modular repair method based on standardized shaping of surface defects, wherein the standardized machining shaping pretreatment of the mold to be repaired is to standardize the damage type and damage level, formulate a standardized machining shaping plan, and process a standardized notch on the mold surface for subsequent laser repair; the specific process is:
[0024] Determine the damage level of the damaged area based on the maximum characteristic size d of the damaged area measured;
[0025] For plane type I damage, the maximum size of the long side of the machining modification is designed as d0; for plane type II damage, the maximum size of the long side of the machining modification is designed as d1; for plane type III damage, the maximum size of the long side of the machining modification is designed as d2;
[0026] For level I edge damage and corner damage, the maximum dimension of the long side of the machining modification is designed as l0; for level II edge damage and corner damage, the maximum dimension of the long side of the machining modification is designed as l1; for level III edge damage and corner damage, the maximum dimension of the long side of the machining modification is designed as l2.
[0027] The laser modular repair method for surface defects based on standardized shaping, wherein the specific process of clamping and positioning the mold to be repaired is: fixing the mold to be repaired on a two-axis positioner and its matching fixed bracket, controlling the rotation direction of the two-axis positioner, and adjusting the angle between the surface to be repaired of the repair mold and the horizontal plane, so that the angle between the normal of the laser processing head and the normal of the surface to be repaired of the mold is controlled between 5° and 10°.
[0028] The laser modular repair method for surface defects based on standardized shaping, wherein the standardized laser repair process is as follows: a database file of each damage type and each damage repair level of the mold to be repaired is embedded into the control software on the industrial computer, and a modular laser automatic repair database for standardized shaping is established according to the damage type and level to be repaired, and the corresponding program file in the database in the control software is selected and exported to the control system of the multi-axis robot, and the modular automatic repair can be realized by running the program file in the automatic control mode.
[0029] The laser modular repair method for surface defects based on standardized shaping, wherein: the database file includes three-dimensional model data, cladding alloy material type, layered slicing data, path planning data and laser parameters; the layered slicing data includes the height value of the layered slicing; the path planning data includes the settings of unidirectional scanning, serpentine scanning, intermittent scanning and interlayer rotation angle; the laser parameters include laser power, scanning speed, overlap rate and interlayer pause time.
[0030] The laser modular repair method based on standardized shaping of surface defects, wherein: after the automated repair of surface defects of different damage types and damage repair levels in the mold to be repaired, the repaired surface can also be machined to reduce its surface roughness.
[0031] By adopting the above technical solution, the present invention has the following beneficial effects:
[0032] The laser modular repair method for surface defects based on standardized shaping of the present invention is reasonably conceived, adopts laser cladding technology, and remanufactures and repairs damaged high-value-added mold surface defects based on a modular repair process database after standardized shaping, thereby improving its mechanical properties such as wear resistance and corrosion resistance.
[0033] The present invention implements standardized shaping from pre-processing, and then implements standardized laser cladding technology, develops serialized and standardized processes, forms a stable process database, reduces the degree of dependence of product quality on experience, and realizes efficient, high-quality and stable mold repair.
[0034] The advantages of the present invention are mainly reflected in the following aspects:
[0035] (1) Before the repair is carried out, the present invention classifies and grades the common damage forms of die steel, sorts out regular and quantifiable damage types and damage levels, and performs standardized machining and shaping pretreatment on the damaged area according to the damage types and damage levels before the repair is carried out. This method is convenient for machining shaping during pretreatment (i.e., standardization and customization of defect machining before repair), and is convenient for the establishment and management of a modular process parameter database during repair. Such a design facilitates the implementation of a standardized laser cladding process, and a serialized and standardized process can be developed;
[0036] (2) The present invention establishes a standardized modular laser automatic repair database to achieve automatic repair of defects of different damage types and damage levels. Since the powder materials, repair objects, and process parameters used in laser cladding are ever-changing, establishing a database to achieve automatic repair can form a stable process database, improve the repair efficiency and consistency of repair quality during batch repairs of enterprises; at the same time, after the database is established, it is easy to manage and maintain the data, and further data mining can be performed based on the established database to select a more universal repair process;
[0037] (3) The present invention is different from Chinese patent CN116352109 A. The present invention is aimed at various defects (i.e., surface defects) appearing on the surface of mold steel, rather than penetrating internal defects appearing on castings. Moreover, Chinese patent CN116352109A uses non-destructive testing technology (X-ray fluoroscopy) to identify and mark the internal defects of the shell casting, which is essentially different from the repair of surface defects in the present invention. Since it is an internal defect, the position of the defect is enclosed by the maximum outer circle in Chinese patent CN116352109A. This defect marking method cannot be applied to defects at the edge / corner position of the present invention. The modular repair in Chinese patent CN116352109A is based on the structure and repair process of the shell martensitic stainless steel casting to divide the shell into different modules, that is, the repair area is the vortex wall area, the flange outlet section, the transition area between the vortex and the outlet section, the U-shaped groove and the root area of the rib plate, and the repair method and process are only aimed at these areas. This is essentially different from the present invention, that is, the present invention is aimed at surface defects. In principle, the repair of any high value-added surface defects can be applied. Using the method of the present invention, secondly, the modular repair of the present invention is not limited to a certain structural part, but belongs to a large category of surface defect repair. The present invention divides defects into surface defects and edge / corner damage, which is a step of classifying defects. The modular repair of the present invention is based on the classification of surface defects and edge / corner defects and is proposed by further probability statistics, and has a wider scope of application; the present invention proposes the concept of a database, that is, the type, grade, repair material, repair process, etc. of the repair defect are embedded in the control software, which is more convenient for standardized management; and the present invention proposes to classify and grade the damage occurring in the mold before repair, perform machining and shaping pretreatment according to the damage condition, form a standard repairable area, and embed the repair process data of the corresponding module into the control software of the industrial computer, so as to realize automatic repair of different damage types and damage levels; that is, to implement standardized shaping from pre-treatment (machining shaping), and then implement standardized laser cladding process, develop serialized and standardized processes, and form a stable process database. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 It is a flow chart of the laser modular repair method of surface defects based on standardized shaping according to the present invention;
[0040] Figure 2The common damage types and locations of the molds involved in the laser modular repair method for standardized surface defects of the present invention ( Figure 2 1- plane damage, 2- right-angle cracks on the edge, 3- missing meat on the corner);
[0041] Figure 3 Schematic diagram of different defect types involved in the laser modular repair method for surface defects based on standardized repair of the present invention ( Figure 3 Figures ab in the figure are schematic diagrams of surface damage, and Figure ce is a schematic diagram of edge / corner damage);
[0042] Figure 4 A physical diagram of the repair process of the laser modular repair method for surface defects based on standardized shaping for implementation of the present invention;
[0043] Figure 5 It is a level II plane damage engineering drawing of standardized shaping involved in the laser modular repair method of surface defects based on standardized shaping of the present invention;
[0044] Figure 6 Schematic diagram of laser cladding path planning for planar level II damage involved in the laser modular repair method for surface defects based on standardized shaping of the present invention ( Figure 6 middle, Figure 6 (a) is a one-way scanning strategy diagram. Figure 6 (b) is a cross scanning strategy diagram);
[0045] Figure 7 This is a laser cladding surface quality map of the plane II level damage involved in the laser modular repair method of the surface defect based on standardized repairing of the present invention ( Figure 7 middle, Figure 7 (a) is a physical picture of the one-way scanning strategy. Figure 7 (b) is a physical picture of the cross-scanning strategy). DETAILED DESCRIPTION
[0046] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] The present invention is further explained below in conjunction with specific implementation modes.
[0048] like Figure 1 As shown, the present embodiment provides a laser modular repair method for surface defects based on standardized shaping, which mainly includes the following steps:
[0049] (1) Classification and grading of mold damage morphology
[0050] Classify the mold according to the probability of damage, such as "lack of meat" on the surface of the part, "pieces falling off" and cracks on the edge, and dents and breakages on the corners, etc., to determine its repairability and sort out regular and quantifiable damage types (the above rules mean: each type of damage has a maximum characteristic size, and the probability distribution characteristics of each defect can be obtained by statistically analyzing the characteristic damage size; the above quantification means: statistically analyzing the damage characteristic size of the damaged mold, classifying it according to the probability of each damage size, and grading the damage based on the statistical results); divide the damage repair level according to the characteristic size and depth of the damaged area. Specifically, the damage defects occurring on the outer surface of the mold are classified into surface damage, edge damage, and corner damage according to the location and shape of the damage ( Figure 2 ), count the actual damage morphology and size of the mold;
[0051] Among them, for planar damage, the following three damage repair levels can be defined:
[0052] Grade I injury: d<d0,
[0053] Grade II injury: d0≤d<d1,
[0054] Grade III injury: d1≤d<d2,
[0055] Among them, d is the maximum characteristic size of the damaged area, d0, d1, and d2 are the maximum sizes under level I, level II, and level III planar damage states respectively obtained based on the probability statistics method; for the case where d is greater than d2, it can be first identified as level III damage, and the damage size of the defective area can be remeasured after repair to determine the repair level, and this cycle is repeated until the repair area is completely coated.
[0056] For edge damage and corner damage, since these two types of damage occur on two intersecting planes, they are classified into the same category and are also divided into three damage repair levels:
[0057] Grade I injury: d<l0,
[0058] Grade II injury: l0≤d<l1,
[0059] Grade III injury: l1≤d<l2,
[0060] l0, l1, and l2 are the maximum dimensions under level I, level II, and level III edge damage and corner damage conditions respectively obtained based on the probability statistics method. For the case where d is greater than l2, it can be first identified as level III damage, and then the damage level of the defective area can be re-judged after repair. This cycle is repeated until the repaired area is completely coated.
[0061] (2) Standardized machining and shaping
[0062] Standardize the damage type and damage level, formulate a standardized machining repair plan, and process standardized notches on the mold surface for subsequent laser repair; the specific process is:
[0063] The damage level is determined based on the maximum characteristic size of the measured damage area. For example, for planar damage, if the maximum characteristic size of the measured damage area is between d0 and d1, it can be determined to be level II damage, and the maximum size of the long side of the machining is designed based on d1 (similarly, for level I damage, it is designed based on d0, and so on). The schematic diagram of the standardized repair machining is shown in the figure. Figure 3 (ab), where Figure 3 a is a cuboid, Figure 3 The cross section of b is an inverted trapezoid, which is recommended when the surface defect is shallow and less than 2 layer thicknesses (usually 1mm). Figure 3 a for machining and shaping, otherwise use Figure 3 b. For edge damage and corner damage, similar methods are used to classify and determine the maximum machining modification size. The schematic diagram of the standardized machining modification of typical edge damage and corner damage is shown in Figure 3 (ce) shown, where Figure 3 (cd) is suitable for areas with damage on the edges. Figure 3 e is suitable for areas with damage on the corners.
[0064] (3) Standardized laser cladding
[0065] (3.1) Clamping and positioning
[0066] Before modular repair, fix the mold to be repaired on a 2-axis positioner and its matching fixed bracket, control the rotation direction of the positioner through the operating handle (the posture angle of the positioner can be adjusted by the program imported into the multi-axis robot control cabinet or manually through the operating handle), and adjust the angle between the surface to be repaired and the horizontal plane, so that the angle between the normal of the laser processing head and the normal of the surface to be repaired is controlled between 5° and 10°.
[0067] (3.2) Laser repair based on standardized process
[0068] A standardized laser repair process is formulated for each type and each level of defect after standardized repair; a database file of each damage type and each damage repair level of the mold to be repaired (the database file mainly includes 3D model data, cladding alloy material type, layered slicing data, path planning data and laser parameters; the cladding alloy material type includes austenitic stainless steel, martensitic stainless steel, nickel-based high-temperature alloy, cobalt-based alloy, H13 steel and other grades of powder materials; the layered slicing data mainly includes the height value of the layered slicing; the path planning data mainly includes path-related data such as unidirectional scanning, serpentine scanning, intermittent scanning, and interlayer rotation angle setting; the laser parameters mainly include laser power, scanning speed, overlap rate, interlayer pause time, etc.) is embedded in the control software on the industrial computer (the control software mainly includes three modules: 3D model, cladding material, and repair process Block; in the "3D model" module of the control software, a 3D model can be established and displayed in the form of a picture to facilitate the experimental operator to select the corresponding repair module. Various brands of materials can be added to the corresponding model. Under specific materials, process-related parameter information can be entered. Some parameters such as scanning paths can also be directly displayed on the interface). According to the type and level of damage to be repaired, a modular laser automatic repair database with standardized repair is established, and the corresponding program file in the database in the control software is selected and transferred to the control system of the multi-axis robot. The program file can be run in automatic control mode to achieve modular automatic repair (the modular repair program already contains the running trajectory, running speed, posture, laser power and other parameters of the multi-axis robot. You only need to select the program to run it to start it with one click, and the repair process will be carried out automatically).
[0069] Among them, after the location and size of defects on the surface of the damaged part are classified and graded according to the above steps (1)-(2), the size and shape of the area to be repaired are determined. The laser repair process parameters of the damaged area under different types, different materials and different characteristic scales are determined through process optimization, and the preferred process data under different damage levels of plane type, edge / corner type are all embedded in the control software of the industrial computer. The data in the software include: standardized repair 3D data map of the damaged area, type of cladding alloy material, layered slicing and path planning data (mainly slicing height, scanning path, overlap spacing and interlayer scanning method, etc.), laser parameters (referring to laser power, scanning speed, interlayer pause time), etc., so as to realize modular management of the repair area, realize automatic repair in batch repair, and improve the consistency and reliability of the repaired products.
[0070] (4) Post-processing such as finishing
[0071] According to the use requirements of the parts, the repaired surface can be further machined, such as grinding, to reduce the surface roughness and improve its use accuracy; such as turning, cutting off a certain depth of the cladding material, etc.
[0072] The present invention will be further described below in conjunction with specific embodiments:
[0073] Embodiment 1:
[0074] The damage of H13 stamping die steel commonly used by a certain enterprise was classified and its damage level was divided into ( Figure 4 A):
[0075] For planar damage, three repair levels are defined based on statistical results, as follows:
[0076] Grade I injury: d < 10 mm,
[0077] Grade II injury: 10mm≤d<30mm,
[0078] Grade III injury: 30mm≤d<50mm,
[0079] Where d is the maximum characteristic size of the damaged area. If d is greater than 50 mm (this is rarely the case in actual repair), it can be identified as Grade III damage first, and the damage level of the defective area can be re-determined after repair, and the cycle is repeated until the repair area is completely coated.
[0080] For edge and corner damage, according to statistical results, they are also divided into three repair levels:
[0081] Grade I injury: d < 5 mm,
[0082] Grade II injury: 5mm≤d<20mm,
[0083] Grade III injury: 20≤d<50mm,
[0084] For cases where d is greater than 50 mm, it can be first identified as Grade III damage, and then the damage level of the defective area can be determined after repair. This cycle is repeated until the repaired area is completely coated.
[0085] The mold surface was then machined and reshaped in a standardized manner. See the schematic diagram of the machined shape for details. Figure 3 , the actual processing picture is as follows Figure 4 B, processed flat type ( Figure 4 B) and corner type ( Figure 4 B), Figure 4 The (ae) in B correspond to Figure 3(ae); clamp the mold and move the multi-axis robot so that the posture and position of the laser processing head are at the set processing position ( Figure 4 C); then, according to the damage type and level of the area to be repaired, select the corresponding program file embedded in the control software (including 3D CAD files, layered slices and path planning data, laser parameters, etc., Figure 4 D), transmitted to the control system of the multi-axis robot, and the program is run in automatic operation mode to realize the automatic repair of the repair area ( Figure 4 E), the quality of the repaired area has good consistency.
[0086] The present invention is further described below by repairing a planar type II damage defect:
[0087] The types of planar defects that are repaired are: Figure 3 As shown in (b), the groove depth is 2 mm, the cross section is an inverted trapezoid, the angle between the side wall and the bottom of the notch is 45°, and it is machined according to the II level plane damage (the maximum surface feature size is 30 mm). The engineering drawing is shown in Figure 5 As shown in the figure (standardized repair pretreatment), the cladding material is H13 steel material with a powder particle size of 53 to 150 μm. The optimized process parameters related to laser repair are: laser power 1500 W, scanning speed 10 mm / s, overlap rate 40%, and scanning strategy is divided into Figure 6 The unidirectional scanning strategy shown in a and Figure 6 The cross scanning strategy (the laser scanning direction of adjacent layers alternates 90°) shown in b was used for three-layer laser cladding experiments. The above important information was embedded in the control software on the industrial computer, and the running program was exported to the control system of the multi-axis robot. After clamping, fixing and positioning the mold to be repaired, the exported program was run in automatic operation mode to achieve automated repair. The actual pictures of the repair effects under different scanning strategies are shown in Figure 7 As shown in the figure, it can be seen that the surface passes of the cladding layer are clearly visible, with metallic luster and good surface flatness. The surface flatness of the unidirectional scanning strategy is better than that of the cross scanning strategy. Therefore, as a repair program in the plane level II damage database, the unidirectional scanning strategy should be preferred for laser repair of the corresponding defects.
[0088] The present invention is rationally conceived, implements standardized shaping from pre-treatment, and then implements standardized laser cladding process, develops serialized and standardized processes, forms a stable process database, reduces the degree of dependence of product quality on experience, and realizes efficient, high-quality and stable mold repair; in particular, the present invention can classify the mold according to the damage situation before repair, determine whether the damaged area is a plane type, edge damage or corner type defect, judge its repairability, and sort out regular and quantifiable damage types; divide the repair level according to the size and depth of the damaged area, standardize the damage type and level, formulate a standardized machining shaping plan, and process standardized notches on the mold surface, which is convenient for machining shaping during pre-treatment and for the establishment and management of a modular process parameter database during repair.
[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A laser modular repair method for surface defects based on standardized shaping, Features: First, the surface damage morphology of the mold to be repaired is classified and graded to sort out regular and quantifiable damage types and damage repair levels; then, the mold to be repaired is pre-treated with standardized machining repair according to the damage type and damage repair level; then, the mold to be repaired after standardized machining repair pre-treatment is clamped and positioned; then, a standardized laser repair process is formulated for surface defects of each damage type and damage repair level in the mold to be repaired after standardized repair; then, a modular laser automatic repair database with standardized repair is established to realize the automated repair of surface defects of different damage types and damage repair levels in the mold to be repaired.
2. The laser modular repair method for surface defects based on standardized shaping as claimed in claim 1, It is characterized in that The process of classifying and grading the damage forms of the mold to be repaired is as follows: The damage defects occurring on the outer surface of the mold are classified into plane damage, edge damage and corner damage according to the location and shape of the damage, and the actual damage shape and size of the mold are counted; For planar damage, the following three levels of damage repair are defined: Grade I injury: d < d 0 , Grade II injury: d 0 ≤d<d 1 , Grade III injury: d 1 ≤d<d 2 , Where d is the maximum characteristic size of the damaged area, d 0 , d 1 , d 2 are the maximum dimensions of the plane damage states of level I, level II, and level III obtained based on the probability statistics method; for d greater than d 2 In the case of a grade III injury, the damage can be identified first. After the repair, the damage size of the defective area is remeasured to determine the repair level. This cycle is repeated until the repaired area is completely coated. The following three levels of damage repair are defined for both edge damage and corner damage: Grade I injury: d<l 0 , Grade II injury: 0 ≤d<l 1 , Grade III injury: l 1 ≤d<l 2 , l 0 , l 1 , l 2 are the maximum dimensions of level I, level II, level III edge damage and corner damage obtained based on the probability statistics method. 2 In the case of a defect, it can be identified as Grade III damage first, and then the damage level of the defect area can be re-evaluated after repair, and the cycle can be repeated until the repair area is completely coated.
3. The laser modular repair method for surface defects based on standardized shaping as claimed in claim 1, Features ,The rule described is that each type of damage has a maximum characteristic size, and the ,probability distribution characteristics of each defect can be obtained by counting the ,characteristic size of this damage; The quantification is as follows: statistically analyzing the characteristic damage dimensions of the damaged mold, classifying each damage dimension according to the probability of occurrence, and grading the damage based on the statistical results.
4. The laser modular repair method for surface defects based on standardized shaping as claimed in claim 1, It is characterized in that The standardized machining and shaping pretreatment of the mold to be repaired is to standardize the damage type and damage level, formulate a standardized machining and shaping plan, and process a standardized notch on the mold surface for subsequent laser repair; the specific process is: Determine the damage level of the damaged area based on the maximum characteristic size d of the damaged area measured; For plane type I damage, the maximum dimension of the long side of the machining modification is d 0 Design; For level II damage of plane type, the maximum dimension of the long side of the machining modification is d 1 Design; For level III damage of plane type, the maximum dimension of the long side of the machining modification is d 2 Conduct design; For level I edge damage and corner damage, the maximum dimension of the long side of the machining modification is l 0 Conduct design; For level II edge damage and corner damage, the maximum dimension of the long side of the machining modification is l 1 Design; For level III edge damage and corner damage, the maximum size of the long side of the machining modification is l 2 Make a design.
5. The laser modular repair method for surface defects based on standardized shaping as claimed in claim 1, It is characterized in that The specific process of clamping and positioning the mold to be repaired is: fix the mold to be repaired on the two-axis positioner and its matching fixed bracket, control the rotation direction of the two-axis positioner, and adjust the angle between the surface to be repaired of the repair mold and the horizontal plane, so that the angle between the normal of the laser processing head and the normal of the surface to be repaired of the mold is controlled between 5° and 10°.
6. The laser modular repair method for surface defects based on standardized shaping as claimed in claim 1, It is characterized in that The standardized laser repair process is as follows: a database file of each damage type and each damage repair level of the mold to be repaired is embedded into the control software on the industrial computer; a standardized modular laser automatic repair database is established according to the damage type and level to be repaired; the corresponding program file in the database in the control software is selected and exported to the control system of the multi-axis robot; and the modular automatic repair can be realized by running the program file in the automatic control mode.
7. The laser modular repair method for surface defects based on standardized shaping as claimed in claim 6, Features: The database file includes three-dimensional model data, cladding alloy material type, layered slice data, path planning data and laser parameters; The layered slice data includes a height value of the layered slice; The path planning data includes the settings of unidirectional scanning, serpentine scanning, intermittent scanning and inter-layer rotation angle; The laser parameters include laser power, scanning speed, overlap rate and inter-layer dwell time.
8. The laser modular repair method for surface defects based on standardized shaping as claimed in claim 1, Features: After the automated repair of surface defects of different damage types and damage repair levels in the mold to be repaired, the repaired surface can also be machined to reduce its surface roughness.
Citation Information
Cited By
Shield tunneling machine hob repairing method and device and medium
CN119703140A
A method, device and medium for repairing a shield machine roller cutter
CN119703140B
Mold composite repair decision-making method and system based on laser heating power layer-by-layer interaction
CN121921436A
Mold composite repair decision method and system based on laser thermal force layer-by-layer interaction
CN121921436B
Radar cover damage classification maintenance method
CN122626505A