Alpine high-altitude field steel rail thermit welding construction method
By fully preheating the rails in high-cold and high-altitude field environments and optimizing the thermite welding process parameters, the problem of excessive cooling of the welded joints was solved, ensuring the standard compliance of the welding quality and the normal use of the rails.
Patent Information
- Application Number
- CN202411031874.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-01
AI Technical Summary
In high-cold and high-altitude outdoor environments, low temperature and lack of oxygen during the rail thermite welding process cause the welded joints to cool too quickly, resulting in welding quality that does not meet standard requirements and a high flaw detection alarm rate, which affects rail production and marketing.
By fully preheating the area near the rail to be welded, thermite welding process parameters are optimized, including using oxyacetylene flame for preheating and sedation, extending the preheating and sedation time, using electric heating induction coils for heating, and connecting acetylene cylinders in series. Wrap the oxygen and acetylene delivery hoses, and use insulation material to wrap the weld area to slow down the cooling rate and ensure even and slow heating.
It effectively reduces the cooling rate after welding, avoids the formation of martensite structure, ensures that the welding quality meets standard requirements, reduces welding defects, and ensures the normal service of the rail.
Smart Images

Figure CN118720320A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rail welding, and in particular to a construction method for thermite welding of rails in the field at high altitudes and cold weather. Background Art
[0002] After the successful development and trial production of new types of rails, it is necessary to complete the welding type inspection and obtain the permission to go on the track before it can be officially put on the track for trial laying. During the track replacement trial laying process, the new type of rail will be welded with the same specification but different type of rails on the existing line. At this time, the best welding method is generally completed by thermite welding. Due to the differences between the environmental factors faced during the construction process and the type inspection, such as the ambient temperature below 0℃, or even minus ten degrees and located in high altitude areas, according to the relevant standards, the rail mobile flash welding operation cannot be carried out. Due to the low rail temperature, low fuel value, too fast cooling speed after welding, and changes in working conditions, the flaw detection alarm rate is high when the welding joint is inspected after welding, and the welding quality does not meet the requirements of relevant standards. The alarm joint needs to be sawed and re-welded, resulting in the inability to complete the welding task within the skylight point on the line, increasing costs, extending the construction period, and the time node for the trial laying of new product rails cannot be guaranteed, which seriously affects the progress of new product development and market promotion of rail production enterprises, thereby causing huge economic losses to enterprises.
[0003] Therefore, it is necessary to study a method that can weld rails using thermite welding in high-cold and high-altitude field environments, and ensure that there is no alarm in the post-weld flaw detection of the rails, that the relevant performance meets the standard requirements, and that the rails can be used in normal service. Summary of the invention
[0004] The main purpose of the present invention is to provide a high-cold and high-altitude outdoor rail aluminothermic welding construction method to solve the technical problem of how to weld rails by aluminothermic welding in a high-cold and high-altitude outdoor environment and ensure the performance of the rails after welding.
[0005] According to one aspect of the present invention, a method for thermite welding of rails in the field at high altitudes and cold weather is provided, comprising: Preheat the entire section of the rail near the area to be welded to a predetermined temperature; The preheated rail is subjected to aluminothermic welding, comprising the following steps in sequence: preheating the rail and the sand mold with an oxyacetylene flame, wherein the oxygen pressure is 0.35-0.45 MPa, the acetylene pressure is 0.04-0.048 MPa, and the preheating time is 360-400 seconds; igniting and pouring the flux; and removing the sand mold after a sedation time of 420-450 seconds.
[0006] According to one embodiment of the present invention, after the sand mold is removed, the tumor pushing operation is performed after 10 to 20 seconds.
[0007] According to one embodiment of the present invention, preheating the entire cross-section of the area near the to-be-welded portion of the rail to a predetermined temperature includes: preheating with an electric heating induction coil.
[0008] According to one embodiment of the present invention, the area near the rail to be welded includes an area extending 200 to 500 mm from the rail to be welded to both sides.
[0009] According to an embodiment of the present invention, the predetermined temperature is 10°C to 15°C.
[0010] According to one embodiment of the present invention, before thermite welding, 8 to 10 acetylene gas cylinders are connected in series using a high-pressure hose.
[0011] According to one embodiment of the present invention, before thermite welding, the acetylene gas cylinder and the oxygen cylinder are placed in a heat preservation environment of 25-30°C.
[0012] According to one embodiment of the present invention, before thermite welding, the oxygen delivery hose and the acetylene delivery hose are wrapped with a heat-insulating material.
[0013] According to one embodiment of the present invention, after the tumor is pushed away, the area near the weld is fully wrapped with a thermal insulation material until the area near the weld is cooled to below 200° C. and then the thermal insulation material is removed.
[0014] According to an embodiment of the present invention, the area near the weld includes an area extending 400 to 500 mm from the weld to both sides.
[0015] In the technical solution of the present invention, on the one hand, the entire section of the rail near the to-be-welded part is preheated, and the rail temperature is increased before welding to reduce the cooling rate of the rail after welding; on the other hand, the process parameters of the thermite welding process are optimized to ensure that the rail is heated evenly and slowly and the heating depth is increased, thereby overcoming the heat loss caused by low temperature and hypoxia in the high-altitude and cold outdoor environment, and further slowing down the cooling rate of the rail welded joint, thereby avoiding the generation of martensitic structure and welding defects, and ensuring that the welding quality meets the requirements of relevant standards and there is no alarm in the post-weld flaw detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 A flow chart of a method for thermite welding of rails in the high-cold and high-altitude field according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0018] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0019] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.
[0020] As mentioned in the above background technology, the inventor of the present application realizes that it is necessary to study a method that can weld rails by aluminothermic welding in a high-cold and high-altitude field environment, and ensure that there is no alarm in the post-weld flaw detection of the rails, the relevant performance meets the standard requirements and can be used in normal service. In order to ensure the construction quality of aluminothermic welding of rails in a high-cold and high-altitude field environment, ensure that there is no alarm in the post-weld flaw detection, and no obvious defects such as low collapse and brittle fracture of welded joints occur during the later service process, the present invention proposes one or more embodiments to be described below, and designs and improves from the measures taken before welding, the matching of welding parameters, the measures taken during welding, and the control of the cooling rate of the joint after welding to ensure the quality of aluminothermic welding of rails in a high-cold and high-altitude field environment. In the embodiment of the present invention, high cold can mean that the ambient temperature is lower than 0°C, and high altitude can mean that the altitude is higher than 1500 meters.
[0021] refer to Figure 1 The present invention proposes a high-cold and high-altitude outdoor rail aluminothermic welding construction method, comprising the following steps: S1, preheating the entire section of the rail near the area to be welded to a predetermined temperature; S2, performing thermite welding on the preheated rail, including the following steps in sequence: preheating the rail and the sand mold with an oxyacetylene flame, wherein the oxygen pressure is 0.35-0.45 MPa, the acetylene pressure is 0.04-0.048 MPa, and the preheating time is 360-400 s; igniting and pouring the flux; and removing the sand mold after a calming time of 420-450 s.
[0022] In the embodiments of the present invention, on the one hand, the whole section of the area near the part to be welded of the rail is preheated, and the rail temperature is increased before welding to reduce the cooling speed of the rail after welding; on the other hand, the process parameters of the thermite welding process are optimized (properly increasing the oxygen pressure and acetylene pressure, extending the preheating time and the sedation time) to ensure that the rail is heated evenly and slowly and the heating depth is increased, so as to overcome the heat loss caused by the low temperature and lack of oxygen in the high-altitude and high-cold field environment, further slow down the cooling speed of the rail welding joint, thereby avoiding the generation of martensitic structure and welding defects, ensuring that the welding quality meets the requirements of relevant standards and that there is no alarm in the post-weld flaw detection. In some solutions of the prior art, liquefied petroleum gas, propane, etc. are used as fuel gas. The present invention has made improvements on this, and uses acetylene with higher fuel value and higher thermal efficiency, which can better adapt to the high-altitude and high-cold field environment.
[0023] In some embodiments, the process of performing thermite welding may include: first, checking the condition of the end of the rail and cleaning the end face of the rail; then, docking the ends of the rails to be welded, adjusting the width of the rail seam, and installing a sand mold so that the end of the rails to be welded is located in the sand mold, and the sand mold may have a shape and size that matches the rail; then, preheating the rail and the sand mold; then, igniting the flux with a high-temperature match, the flux may include aluminum powder and iron oxide (in order to adjust the molten metal temperature and the chemical composition of the weld metal, an appropriate amount of additives and alloys may be added to the flux), placing it in a crucible, and igniting it. After that, thermite reaction occurs and a large amount of heat is released, resulting in liquid metal (such as molten iron) and slag (mainly Al2O3). The liquid metal has a high density and sinks to the bottom of the crucible, while the slag is light and floats on the top. Then the liquid metal is poured into the sand mold, and the liquid metal flows into the joint gap to form the weld metal. After the pouring is completed, the sand mold is removed after a predetermined calming time. During the calming time, the liquid metal gradually solidifies to connect the two sections of rails as a whole. After that, the excess part of the weld joint can be pushed away with a pusher, and the weld joint can be polished after cooling. Thermite welding has the advantages of simple equipment, easy use, and no need for power supply.
[0024] In some embodiments, after the sand mold is removed, the knob pushing operation is performed after 10 to 20 seconds, and this interval time is beneficial to further reduce the cooling rate of the rail.
[0025] In some embodiments, the area near the rail to be welded includes an area extending 200 to 500 mm on both sides of the rail to be welded, and the predetermined temperature is 10°C to 15°C to ensure the required preheating effect and prepare for subsequent welding.
[0026] Various feasible heating means can be used to preheat the area near the part of the rail to be welded. In some embodiments, the entire cross-section of the area near the part of the rail to be welded is preheated to a predetermined temperature, including: preheating with an electric heating induction coil. The induction coil is connected to a power supply and is arranged on the periphery of the rail. The power supply provides an alternating current to the coil. The alternating current flowing through the coil generates an alternating magnetic field passing through the rail. The magnetic field causes the rail to generate eddy currents for heating. By adopting the induction coil heating method, the area near the part to be welded can be preheated quickly and evenly, greatly improving the working efficiency. The induction coil heating method can be used by preparing a small generator with the engineering vehicle, which is convenient to use. The induction coil can have a shape that matches the rail.
[0027] In some embodiments, before performing thermite welding, 8 to 10 acetylene gas cylinders are connected in series using high-pressure hoses to increase the total gas supply, improve the fuel value, ensure the continuity of the preheating process, and improve the preheating effect.
[0028] In some embodiments, before thermite welding, the acetylene cylinder and the oxygen cylinder are placed in a heat preservation environment of 25-30°C to prevent the acetylene and oxygen temperatures from being too low and affecting the provision of the oxyacetylene flame. During the preheating of the rails and the sand mold, the acetylene cylinder and the oxygen cylinder can always be placed in a heat preservation environment. For example, the acetylene cylinder and the oxygen cylinder can be loaded in the compartments of two engineering vehicles respectively, and air conditioners can be installed in the compartments of the two engineering vehicles, and the temperature is set to 25-30°C.
[0029] In some embodiments, before thermite welding, the oxygen delivery hose and the acetylene delivery hose are wrapped with a heat-insulating material, so that during the preheating of the rail and the sand mold, the oxygen delivery hose and the acetylene delivery hose are insulated by the heat-insulating material, further maintaining the temperature of oxygen and acetylene and reducing heat loss. For example, a heat-insulating blanket can be used to wrap the oxygen delivery hose and the acetylene delivery hose.
[0030] By connecting multiple acetylene cylinders in series and providing all-round insulation for acetylene cylinders, oxygen cylinders, oxygen delivery hoses and acetylene delivery hoses, it is possible to overcome the problems of low fuel value and incomplete combustion caused by high altitudes, as well as the problem of condensation of oxygen delivery hoses and acetylene delivery hoses during use due to extremely cold weather, resulting in low flame energy or even interruption of the combustion process.
[0031] In some embodiments, after the push-up is completed, the area near the weld is fully wrapped with insulation material until the area near the weld is cooled to below 200°C and then the insulation material is removed. By wrapping the area near the weld with insulation material, the weld joint can be prevented from cooling too fast and forming harmful martensitic structure. The area near the weld may include an area extending 400 to 500 mm from the weld to both sides. For example, after the push-up is completed, an insulation blanket is used to fully wrap the 500 mm range on both sides of the weld until it is slowly cooled to below 200°C and then the insulation blanket is removed, and then the entire section is polished.
[0032] The following is an explanation based on specific embodiments and comparative examples.
[0033] Example 1 The rail temperature of this embodiment is -8℃, the altitude is 3800m, and the working window period is around 22:00 at night. During the preparation work, 8 acetylene cylinders are connected in series with gas high-pressure hoses to increase the total gas supply and improve the thermal efficiency of combustion. The engineering flatbed car loaded with acetylene cylinders is equipped with an air conditioner with a set temperature of 25℃. The oxygen cylinder is carried by another engineering car compartment, and the air conditioner is also set to 25℃ in the compartment. The oxygen delivery hose and acetylene delivery hose are wrapped with an insulation blanket. Before welding, an electric heating induction coil is used to preheat the entire section within 200mm on both sides of the steel rail to be welded, and the preheating temperature is 10℃, and the sand mold and crucible are evenly heated to remove moisture and dry them. After the preheating before welding is completed, the sand mold is installed, and then the rail and sand mold are preheated with an oxyacetylene flame, wherein the oxygen pressure is 0.35MPa, the acetylene pressure is 0.04MPa, and the preheating time is 370s. After that, the flux is ignited and poured. After pouring, the sand mold is removed after a 430s cooling time. After the sand mold is removed, the nodule is pushed after 10s. After the nodule is pushed, the insulation blanket is used to wrap the entire section within 500mm on both sides of the weld until it is slowly cooled to below 200℃, then the insulation blanket is removed and the entire section is polished. After polishing, ultrasonic flaw detection is used, and the result is no damage. No collapse or broken rails have occurred after the opening to traffic.
[0034] Example 2 The rail temperature of this embodiment is -15℃, the altitude is 4500m, and the working window period is at night and early morning. During the preparation work, 10 acetylene cylinders are connected in series using gas high-pressure hoses to increase the total gas supply and improve the thermal efficiency of combustion. An air conditioner is installed in the engineering flatbed car loaded with acetylene cylinders, and the temperature is set to 30℃. The oxygen cylinder is carried by another engineering car compartment, and the air conditioner is also set to 30℃ in the compartment. The oxygen delivery hose and acetylene delivery hose are wrapped with insulation blankets. Before welding, an electric heating induction coil is used to preheat the entire section within 500mm on both sides of the steel rail to be welded, and the preheating temperature is 10℃, and the sand mold and crucible are evenly heated to remove moisture and dry them. After the preheating before welding is completed, the sand mold is installed, and then the rail and sand mold are preheated with an oxyacetylene flame, wherein the oxygen pressure is 0.4MPa, the acetylene pressure is 0.048MPa, and the preheating time is 400s. After that, the flux is ignited and poured. After pouring, the sand mold is removed after a 450s cooling time. After the sand mold is removed, the nodule is pushed after 20s. After the nodule is pushed, the insulation blanket is used to wrap the entire section within 500mm on both sides of the weld until it is slowly cooled to below 200℃, then the insulation blanket is removed and the entire section is polished. After polishing, ultrasonic flaw detection is used, and the result is no damage. No collapse or broken rails have occurred after the opening to traffic.
[0035] Comparative Example 1 The rail temperature of this comparative example is -8℃, the altitude is 3800m, and the working skylight period is around 22:00 at night. The welding construction process is: rust removal and decontamination of rail ends, removal of water stains → rail alignment → installation of sand molds → fixture installation → sealing → preheating → installation of crucibles → ignition → reaction → demolding → pushing tumors → grinding → flaw detection. After welding, the whole section is polished and then ultrasonic flaw detection is used. The result is serious damage. Another skylight point saw is applied for and a 6m short rail is inserted. The temporary measure of drilling and then putting on the splint is adopted to ensure the normal operation of the line, and the rail replacement welding will be carried out again when the opportunity is selected.
[0036] Comparative Example 2 The rail temperature of this comparative example is -15℃, the altitude is 4500m, and the working skylight period is at night and early morning. The welding construction process is: wipe the water stains on the end of the rail with dry cotton yarn → grind and remove rust from the rail end → align the rail → install the sand mold → install the fixture → seal the box → preheat → install the crucible → ignite → react → remove the mold → push the tumor → grind → flaw detection. After welding, the whole section is polished and then ultrasonic flaw detection is used. The result is serious damage. Another skylight point saw is applied for and a short rail is inserted. The temporary measure of punching the upper splint is adopted to ensure the normal operation of the line, and the rail replacement welding will be carried out again when the opportunity is selected.
[0037] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for thermite welding of rails in the field at high altitudes and cold weather, characterized in that: include: Preheating the entire section of the rail near the area to be welded to a predetermined temperature; The preheated rail is subjected to aluminothermic welding, comprising the following steps in sequence: preheating the rail and the sand mold by using an oxyacetylene flame, wherein the oxygen pressure is 0.35-0.45 MPa, the acetylene pressure is 0.04-0.048 MPa, and the preheating time is 360-400 seconds; igniting and pouring the flux; and removing the sand mold after a sedation time of 420-450 seconds.
2. The method according to claim 1, characterized in that: After removing the sand mold, wait 10 to 20 seconds before pushing the tumor away.
3. The method according to claim 1, characterized in that The method of preheating the entire cross-section of the area near the to-be-welded portion of the rail to a predetermined temperature includes: preheating with an electric heating induction coil.
4. The method according to claim 1, characterized in that: The area near the rail to be welded includes an area extending 200 to 500 mm to both sides of the rail to be welded.
5. The method according to claim 1, characterized in that The predetermined temperature is 10°C to 15°C.
6. The method according to claim 1, characterized in that Before the above-mentioned thermite welding, 8 to 10 acetylene gas cylinders are connected in series using high-pressure hoses.
7. The method according to claim 1, characterized in that Before the aluminothermic welding, the acetylene gas cylinder and the oxygen cylinder are placed in a heat preservation environment of 25-30°C.
8. The method according to claim 1, characterized in that Before the thermite welding, the oxygen delivery hose and the acetylene delivery hose are wrapped with a heat-insulating material.
9. The method according to claim 2, characterized in that: After the tumor is pushed away, the area near the weld is fully wrapped with insulation material until the area near the weld is cooled to below 200° C. and then the insulation material is removed.
10. The method according to claim 9, characterized in that The area near the weld includes an area extending 400 to 500 mm from the weld to both sides.