Gas shielded welding process suitable for welding Ni series steel and 316L dissimilar steel
Through the gas shielded welding process and specific welding parameters, the problem of low-temperature impact toughness and mechanical properties of the welded joints of Ni series steel and 316L dissimilar steel was solved, and excellent comprehensive mechanical properties of the welded joints were achieved to meet market standards.
Patent Information
- Application Number
- CN202410846621.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
Smart Images

Figure CN118720340A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel production, and in particular to a gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel. Background Art
[0002] Ni-based steel is used for LNG tanks. In addition to the tank body itself, LNG tanks also need to be connected to feed pipes, accessories, etc. during construction. Generally, 316L stainless steel is used, which involves the connection of dissimilar materials. Ni-based steel and 316L dissimilar steel are connected by welding technology to form a structure used for storing and transporting cryogenic storage tanks. Whether the welding of this dissimilar steel has a wide welding process window, and whether the joint performance after welding, especially the low-temperature impact toughness of the welded joint, can meet the standards or user requirements, has become the first threshold for this type of steel to enter the market. Therefore, it is necessary to develop a gas shielded welding process suitable for the welding of Ni-based steel and 316L dissimilar steel, and to weld Ni-based steel and 316L dissimilar steel by gas shielded welding to ensure that the mechanical properties of the welded joint meet the requirements. Summary of the invention
[0003] The technical problem to be solved by the present invention is to overcome the disadvantages of the prior art and provide a gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel.
[0004] In order to solve the above technical problems, the technical solution of the present invention is as follows: A gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel, comprising: Use gas shielded welding to connect Ni-based steel and 316L dissimilar steel with welding wire; A symmetrical X-shaped groove is used as the arc welding groove, with a groove angle of 55°-65°, a blunt edge length of 1mm-3mm, and a groove assembly clearance of 1mm-3mm; No preheating before welding, the interlayer temperature is less than or equal to 120℃, and the back side is cleaned before welding; Gas shielded welding is used with a welding current of 280A-350A, an arc voltage of 21V-25V, a welding speed of 32cm / min-38cm / min, and a welding heat input of 10kJ / cm-16kJ / cm until the welding is completed.
[0005] As a preferred scheme of the gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, the chemical composition and mass percentage of the Ni-based steel are as follows: C: 0.045%-0.060%, Mn: 0.50%-1.50%, Si: 0.10%-0.30%, S: ≤0.01%, P: ≤0.01%, Ni: 6.50%-8.00%, Mo: 0.20%-0.40%, and the balance is Fe and unavoidable impurities.
[0006] As a preferred solution of the gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, wherein: the yield strength of the Ni-based steel is ≥580MPa, the tensile strength is ≥680MPa-820MPa, the elongation is ≥18%, and the impact energy KV2 at -196°C is ≥100J.
[0007] As a preferred solution of the gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, the thickness of the Ni-based steel is 16mm-40mm.
[0008] As a preferred scheme of the gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, the chemical composition and mass percentage of the 316L dissimilar steel are as follows: C: ≤0.04%, Mn: 0.50%-2.50%, Si: ≤0.90%, S: ≤0.02%, P: ≤0.03%, Ni: 11.0%-14.0%, Cr: 17.0%-20.0%, Mo: 0.3%-0.7%, Cu: ≤0.75%, and the balance is Fe and unavoidable impurities.
[0009] As a preferred solution of the gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, wherein: the yield strength of the 316L dissimilar steel is ≥177MPa, the tensile strength is ≥480MPa, the elongation is ≥40%, and the impact energy KV2 at -196℃ is ≥34J.
[0010] As a preferred scheme of the gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, the chemical composition and mass percentage of the welding wire are as follows: C: 0.20%-0.35%, Mn: 9.0%-11.0%, Si: 0.42%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~18%, W: 4.0%~6.0%, and the balance is Fe and unavoidable impurities.
[0011] As a preferred solution of the gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, the welding wire is a gas shielded welding wire with a diameter of 1.2 mm, the low-temperature impact energy of the deposited metal at -196°C KV2≥48J, and the tensile strength≥600Mpa.
[0012] As a preferred solution of the gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, wherein: after the gas shielded welding is completed, the low-temperature impact energy of the weld joint at -196°C KV2≥34J, the tensile strength of the weld joint≥480Mpa, the longitudinal surface bend d=4a, and 180° of the weld joint is qualified.
[0013] The beneficial effects of the present invention are: The gas shielded welding process provided by the invention is easy to operate and can ensure that the low-temperature impact energy KV2 of the welded joint (weld and heat-affected zone) at -196°C is ≥34J, the tensile strength of the welded joint is ≥480Mpa, and the longitudinal bend of the welded joint is d=4a, 180° is qualified. The welded joint formed by the welding process has good comprehensive mechanical properties and is suitable for welding 16mm-40mm thick Ni-series steel and 316L dissimilar steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.
[0015] Figure 1 Schematic diagram of welding Ni-based steel and 316L dissimilar steel provided by the present invention. DETAILED DESCRIPTION
[0016] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific implementation modes and in combination with the accompanying drawings.
[0017] The embodiment of the present application provides a gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel, the process comprising the following steps: Step S101: Connect Ni-based steel and 316L dissimilar steel with welding wire in a gas shielded welding manner.
[0018] Specifically, the chemical composition and mass percentage of Ni-based steel are as follows: C: 0.045%-0.060%, Mn: 0.50%-1.50%, Si: 0.10%-0.30%, S: ≤0.01%, P: ≤0.01%, Ni: 6.50%-8.00%, Mo: 0.20%-0.40%, and the balance is Fe and unavoidable impurities.
[0019] Among them, the yield strength of Ni-based steel is ≥580MPa, the tensile strength is ≥680MPa-820MPa, the elongation is ≥18%, and the impact energy KV2 at -196℃ is ≥100J.
[0020] It should be noted that the present application is applicable to Ni-based steel with a thickness of 16 mm to 40 mm.
[0021] The chemical composition and mass percentage of 316L dissimilar steel are as follows: C: ≤0.04%, Mn: 0.50%-2.50%, Si: ≤0.90%, S: ≤0.02%, P: ≤0.03%, Ni: 11.0%-14.0%, Cr: 17.0%-20.0%, Mo: 0.3%-0.7%, Cu: ≤0.75%, the balance is Fe and unavoidable impurities.
[0022] Among them, the yield strength of 316L heterogeneous steel is ≥177MPa, the tensile strength is ≥480MPa, the elongation is ≥40%, and the impact energy KV2 at -196℃ is ≥34J.
[0023] The chemical composition and mass percentage of the welding wire are as follows: C: 0.20%-0.35%, Mn: 9.0%-11.0%, Si: 0.42%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~18%, W: 4.0%~6.0%, and the balance is Fe and unavoidable impurities.
[0024] Among them, the welding wire is a gas shielded welding wire with a diameter of 1.2mm, the low-temperature impact energy of the deposited metal at -196℃ KV2≥48J, and the tensile strength≥600Mpa.
[0025] It should be noted that when selecting welding materials, the first consideration is to obtain a complete weld joint and ensure that the low-temperature impact energy of the weld joint at -196℃ KV2 ≥ 34J and the tensile strength of the weld joint ≥ 480MPa.
[0026] Step S102: using a symmetrical X-shaped groove as the arc welding groove, with a groove angle of 55°-65°, a blunt edge length of 1mm-3mm, and a groove assembly clearance of 1mm-3mm.
[0027] Step S103: No preheating before welding, the interlayer temperature is less than or equal to 120° C., and root cleaning is performed before reverse side welding.
[0028] Step S104: gas shielded welding is used, with a welding current of 280A-350A, an arc voltage of 21V-25V, a welding speed of 32cm / min-38cm / min, and a welding heat input of 10kJ / cm-16kJ / cm, until the welding is completed.
[0029] The gas shielded welding process applicable to the welding of Ni-based steel and 316L dissimilar steel is described below through a specific embodiment.
[0030] Embodiment 1: The gas shielded welding process for welding Ni-based steel and 316L dissimilar steel provided in this embodiment comprises the following steps: The parent material is Ni-series steel with yield strength ≥580MPa, tensile strength ≥680MPa-820MPa, elongation ≥18%, and impact energy KV2 ≥100J at -196℃, and 316L with yield strength ≥177MPa, tensile strength ≥480MPa, elongation ≥40%, and impact energy KV2 ≥34J at -196℃, for butt welding. The welding test plate combination is 16mm+16mm, and the test plate size is 500mm (length) × 200mm (width) × 16mm (thickness).
[0031] The welding material is a gas shielded welding wire with a diameter of Φ1.2mm. The deposited metal has a low-temperature impact energy of -196℃ KV2≥48J and a tensile strength≥600MPa. The welding wire includes the following components in weight percentage: C: 0.20%-0.35%, Mn: 9.0%-11.0%, Si: 0.42%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~18%, W: 4.0%~6.0%, and the balance is Fe and unavoidable impurities.
[0032] The groove type is X-shaped groove, the groove angle is 55°, the blunt edge is 1mm, and the groove assembly clearance is 1mm.
[0033] No preheating before welding, the interlayer temperature is 30℃-90℃; the root is cleaned with a grinder before welding on the reverse side, and the root has a metallic luster.
[0034] Gas shielded welding was used with a welding current of 210A, an arc voltage of 25V, a welding speed of 30cm / min, a welding heat input of 10kJ / cm, a shielding gas of 98%Ar+2%O2 gas, and a gas flow rate of 15L / min until the welding was completed.
[0035] Embodiment 2: The gas shielded welding process applicable to the welding of Ni-based steel and 316L dissimilar steel of this embodiment comprises the following steps: The parent material is Ni-series steel with yield strength ≥580MPa, tensile strength ≥680MPa-820MPa, elongation ≥18%, and impact energy KV2 ≥100J at -196℃, and 316L with yield strength ≥177MPa, tensile strength ≥480MPa, elongation ≥40%, and impact energy KV2 ≥34J at -196℃ for butt welding. The welding test plate combination is 30mm+30mm, and the test plate size is 500mm (length) × 200mm (width) × 30mm (thickness).
[0036] The welding material is a gas shielded welding wire with a diameter of Φ1.2mm. The deposited metal has a low-temperature impact energy of -196℃ KV2≥48J and a tensile strength≥600MPa. The welding wire includes the following components in weight percentage: C: 0.20%-0.35%, Mn: 9.0%-11.0%, Si: 0.42%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~18%, W: 4.0%~6.0%, and the balance is Fe and unavoidable impurities.
[0037] The groove type is X-shaped groove, the groove angle is 58°, the blunt edge is 2mm, and the groove assembly clearance is 1mm.
[0038] No preheating before welding, the interlayer temperature is 31℃-87℃; the root is cleaned with a grinder before welding on the reverse side, and the root has a metallic luster.
[0039] Submerged arc welding was used with a welding current of 240A, an arc voltage of 26V, a welding speed of 28cm / min, a welding heat input of 13kJ / cm, a shielding gas of 98%Ar+2%O2 gas, and a gas flow rate of 16L / min until the welding was completed.
[0040] Embodiment 3: The gas shielded welding process applicable to the welding of Ni-based steel and 316L dissimilar steel of this embodiment comprises the following steps: The parent material is Ni-series steel with yield strength ≥580MPa, tensile strength ≥680MPa-820MPa, elongation ≥18%, and impact energy KV2 ≥100J at -196℃, and 316L with yield strength ≥177MPa, tensile strength ≥480MPa, elongation ≥40%, and impact energy KV2 ≥34J at -196℃. The welding test plate combination is 40mm+40mm, and the test plate size is 500mm (length) × 200mm (width) × 40mm (thickness).
[0041] The welding material is a gas shielded welding wire with a diameter of Φ1.2mm. The deposited metal has a low-temperature impact energy of -196℃ KV2≥47J and a tensile strength≥660MPa. The welding wire includes the following components in weight percentage: C: 0.20%-0.35%, Mn: 9.0%-11.0%, Si: 0.42%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~18%, W: 4.0%~6.0%, and the balance is Fe and unavoidable impurities.
[0042] The groove type is X-shaped groove, the groove angle is 60°, the blunt edge is 1mm, and the groove assembly clearance is 1mm.
[0043] No preheating before welding, the interlayer temperature is 33℃-92℃; the root is cleaned with a grinder before welding on the reverse side, and the root has a metallic luster.
[0044] Gas shielded welding was used with a welding current of 260A, an arc voltage of 30V, a welding speed of 26cm / min, a welding heat input of 18kJ / cm, a shielding gas of 98%Ar+2%O2 gas, and a gas flow rate of 15L / min until the welding was completed.
[0045] The Ni-based steel and 316L dissimilar steel were welded by the welding method of the above-mentioned Examples 1-3, and the mechanical properties of the welded joints were tested. The impact, tensile and bending properties of the welded joints are shown in Tables 1 and 2:
[0046] Table 1: Impact performance of welded joints
[0047] Table 2: Tensile and lateral bending properties of welded joints It can be seen from Table 1 and Table 2 that the comprehensive mechanical properties of the welded joints obtained in Examples 1-3 are excellent. The impact energy of the weld and the heat-affected zone at -196°C KV2≥34J, the tensile strength Rm:≥480MPa, the longitudinal bend of the welded joint d=4a, 180° is qualified, and the process implementation method provided is simple and highly applicable.
[0048] Therefore, the technical solution provided by the present application is not only easy to operate, but also the welded joint formed by the welding process has good comprehensive mechanical properties.
[0049] In addition to the above embodiments, the present invention may also have other implementation modes; any technical solutions formed by equivalent replacement or equivalent transformation shall fall within the protection scope required by the present invention.
Claims
1. A gas shielded welding process suitable for welding Ni-based steel and 316L dissimilar steel. Features: include: Use gas shielded welding to connect Ni-based steel and 316L dissimilar steel with welding wire; A symmetrical X-shaped groove is used as the arc welding groove, with a groove angle of 55°-65°, a blunt edge length of 1mm-3mm, and a groove assembly clearance of 1mm-3mm; No preheating before welding, the interlayer temperature is less than or equal to 120℃, and the back side is cleaned before welding; Gas shielded welding is used with a welding current of 280A-350A, an arc voltage of 21V-25V, a welding speed of 32cm / min-38cm / min, and a welding heat input of 10kJ / cm-16kJ / cm until the welding is completed.
2. The gas shielded welding process for welding Ni-based steel and 316L dissimilar steel according to claim 1, Features: The chemical composition and mass percentage of the Ni-based steel are as follows: C: 0.045%-0.060%, Mn: 0.50%-1.50%, Si: 0.10%-0.30%, S: ≤0.01%, P: ≤0.01%, Ni: 6.50%-8.00%, Mo: 0.20%-0.40%, and the balance is Fe and unavoidable impurities.
3. The gas shielded welding process for welding Ni-based steel and 316L dissimilar steel according to claim 2, Features: The yield strength of the Ni-based steel is ≥580MPa, the tensile strength is ≥680MPa-820MPa, the elongation is ≥18%, and the impact energy KV at -196℃ 2 ≥100J.
4. The gas shielded welding process for welding Ni-based steel and 316L dissimilar steel according to claim 1, Features: The thickness of the Ni-based steel is 16 mm to 40 mm.
5. The gas shielded welding process for welding Ni-based steel and 316L dissimilar steel according to claim 1, Features: The chemical composition and mass percentage of the 316L heterogeneous steel are as follows: C: ≤0.04%, Mn: 0.50%-2.50%, Si: ≤0.90%, S: ≤0.02%, P: ≤0.03%, Ni: 11.0%-14.0%, Cr: 17.0%-20.0%, Mo: 0.3%-0.7%, Cu: ≤0.75%, and the balance is Fe and unavoidable impurities.
6. The gas shielded welding process for welding Ni-based steel and 316L dissimilar steel according to claim 5, Features: The yield strength of the 316L heterogeneous steel is ≥177MPa, the tensile strength is ≥480MPa, the elongation is ≥40%, and the impact energy KV at -196℃ 2 ≥34J.
7. The gas shielded welding process for welding Ni-based steel and 316L dissimilar steel according to claim 1, Features: The chemical composition and mass percentage of the welding wire are as follows: C: 0.20%-0.35%, Mn: 9.0%-11.0%, Si: 0.42%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~18%, W: 4.0%~6.0%, and the balance is Fe and unavoidable impurities.
8. The gas shielded welding process for welding Ni-based steel and 316L dissimilar steel according to claim 7, Features: The welding wire is a gas shielded welding wire with a diameter of 1.2 mm, and the deposited metal has a low-temperature impact energy of KV 2 ≥48J, tensile strength ≥600Mpa.
9. The arc welding process for welding Ni-based steel and 316L dissimilar steel according to claim 1, Features: After the gas shielded welding is completed, the weld joint has a low-temperature impact energy of -196℃ KV 2 ≥34J, tensile strength of welded joint ≥480Mpa, longitudinal bend of welded joint d=4a, 180° qualified.
Citation Information
Patent Citations
Welding method for high manganese steel and 316L dissimilar steel
CN116352235A
Submerged-arc welding process for marine-corrosion-resistant steel with yield strength of 420 MPa
CN117206643A
Submerged arc welding process suitable for welding high manganese steel and 316L dissimilar steel
CN117483926A
Submerged-arc welding process suitable for welding high-manganese steel and 9Ni dissimilar steel