Flux-cored welding rod for surfacing repair
By using a core layer of high-carbon ferrochrome and a coating layer of calcium fluoride and other materials in the surfacing repair material, combined with the design of the aluminum mesh, the problem of balancing high hardness and high toughness of the surfacing layer is solved , achieving the welding effect of high hardness and high toughness, improving the service life and welding quality of the BD roll.
Patent Information
- Application Number
- CN202410882637.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-01
AI Technical Summary
Existing surfacing repair materials are difficult to balance between high hardness and high toughness, causing the BD roll to easily crack or peel off during use.
It adopts a core layer composed of high carbon ferrochrome, molybdenum powder, ferrovanadium, niobium powder, manganese powder, aluminum powder and iron powder, combined with low carbon steel strip and calcium fluoride, titanium powder, magnesium oxide, calcium carbonate, etc. The coating layer of the material, and an aluminum mesh is set inside the coating layer to form a high alkalinity environment to improve the toughness and wear resistance of the surfacing layer.
It achieves both high hardness and high toughness of the cladding layer, reduces the content of P, S, O, and H, and forms a uniformly distributed high-carbon martensite base plus dispersion structure, which improves the welding quality and the service life of the roll.
Smart Images

Figure CN118720515A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding materials, and in particular to a flux-cored welding rod for surfacing repair. Background Art
[0002] BD rollers are the most important hot tools for rail and profile production lines. In addition to normal wear, BD rollers are also damaged by fatigue cracks and peeling of roller surfaces during use. Therefore, repairing BD rollers by surfacing welding can not only save a lot of spare parts costs, achieve considerable economic benefits, and save a lot of energy and resources.
[0003] Flux-cored welding wires used for cladding repair of metallurgical hot rolling rollers are mostly made of Cr5-based alloys, and then different Mo, W, V, Co, Nb and other alloys are added to strengthen them. The hardness of the cladding layer is about HRc50. After the cladding roller is installed on the machine, it can basically meet the working requirements of the rolling mill, but the wear resistance of the cladding layer is not ideal, mainly because the cladding layer is not strong enough. This is because when the hardness of the cladding working layer is >50HRc, the toughness of the material will be greatly reduced, and the BD roller is very likely to crack or peel off during cladding or use.
[0004] Therefore, the problem existing in the prior art is: how to ensure high hardness and high toughness of the cladding layer. Summary of the invention
[0005] The invention provides a flux-cored welding rod for surfacing repair, aiming to provide a welding rod with high hardness and high toughness when repairing a rolling mill roll.
[0006] The technical solution used in the present invention is as follows:
[0007] A flux-cored welding rod for surfacing repair comprises a steel strip and a first flux-core layer and a second flux-core layer wrapped inside the steel strip.
[0008] The first core layer and the second core layer have the same composition, and the first core layer and the second core layer are composed of the following raw materials in percentage by mass: 25%-35% high carbon ferrochrome; 5%-10% molybdenum powder; 1%-5% ferrovanadium; 9%-15% niobium powder; 5%-7% manganese powder, 3%-4% aluminum powder; the remainder is iron powder, and the sum of each component is 100%;
[0009] The particle size of the first drug core layer is greater than the particle size of the second drug core layer.
[0010] Furthermore, the steel belt is made of low carbon steel HS1 steel belt, the thickness of the steel belt is 0.3-0.8 mm, and the diameter of the cylinder surrounded by the steel belt is 2.8 mm-4.0 mm.
[0011] Furthermore, the volume ratio of the first drug core layer to the second drug core layer is 2:2.5-3.5; the particle size of the first drug core layer is 160 mesh-200 mesh, and the particle size of the second drug core layer is 120 mesh-160 mesh.
[0012] Furthermore, the volume ratio of the first drug core layer to the second drug core layer is 2:3; the particle size of the first drug core layer is 180 mesh, and the particle size of the second drug core layer is 140 mesh.
[0013] Furthermore, a coating layer is provided on the outside of the steel strip, and the coating layer is composed of the following raw materials in percentage by mass: 30% to 40% calcium fluoride, 35% to 45% titanium powder, 15% to 25% magnesium oxide, and 4% to 6% calcium carbonate, and the sum of the components is 100%.
[0014] Furthermore, an aluminum mesh is provided in a ring shape on the outer side of the steel strip and the inner side of the coating layer.
[0015] Furthermore, the mesh size of the aluminum mesh is 20-80 meshes, and the thickness of the aluminum mesh is 0.2 mm-0.8 mm.
[0016] Furthermore, the drug skin layer is composed of the following raw materials in percentage by mass: 35% calcium fluoride, 40% titanium powder, 20% magnesium oxide, and 5% calcium carbonate.
[0017] The beneficial effects achieved by the present invention are as follows: the coating on the outer side of the steel strip plays a protective role, wherein calcium fluoride can generate a large amount of gas to cover the arc and the molten pool, playing a role of isolating the air, so that the molten metal formed inside the welding rod will not interact with the air; the first flux core layer and the second flux core layer match the high alkalinity environment formed by calcium fluoride, and the P, S, O, and H contents in the obtained cladding layer are low, and the structure is a high-carbon martensite base plus dispersed and evenly distributed carbon, nitride and a small amount of ferrite. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The structure of the flux-cored electrode for surfacing welding repair of the present invention is schematically shown. Figure 1 .
[0019] Figure 2 The structure of the flux-cored electrode for surfacing welding repair of the present invention is schematically shown. Figure 2 .
[0020] Figure 3 This is a microstructure photograph of the welding wire cladding layer produced in Example 2 of the present invention.
[0021] In the figure, 1, steel strip; 2, first core layer; 3, second core layer; 4, skin layer; 5, aluminum mesh. DETAILED DESCRIPTION
[0022] To facilitate those skilled in the art to understand the present invention, specific implementations of the present invention are described below with reference to the accompanying drawings.
[0023] like Figure 1As shown, the present invention provides a flux-cored electrode for surfacing repair, comprising a steel strip and a first flux-cored layer and a second flux-cored layer wrapped inside the steel strip.
[0024] The steel strip is low-carbon steel HS1 steel strip with a thickness of 0.3-0.8 mm and a cylindrical diameter of 2.8 mm-4.0 mm. The composition (mass percentage) of the first core layer and the second core layer are both high-carbon ferrochrome 25%-35%; molybdenum powder 5%-10%; ferrovanadium 1%-5%; niobium powder 9%-15%; manganese powder 5%-7% and aluminum powder 3%-4%; iron powder is the remainder, and the sum of each component is 100%.
[0025] The volume ratio of the first drug core layer to the second drug core layer is 2:2.5-3.5; the particle size of the first drug core layer is 160 mesh-200 mesh, and the particle size of the second drug core layer is 120 mesh-160 mesh.
[0026] During welding, molten metal is formed inside the electrode, which will interact with the air, thus affecting the welding quality; a coating layer is provided on the outside of the steel strip, and the coating layer is composed of the following raw materials in percentage by mass: 30% to 40% calcium fluoride, 35% to 45% titanium powder, 15% to 25% magnesium oxide, 4% to 6% calcium carbonate, and the sum of the components is 100%;
[0027] During the welding process, the coating on the outside of the steel strip plays a protective role. Calcium fluoride can produce a large amount of gas to cover the arc and the molten pool, which plays a role in isolating the air. In this way, the molten metal formed inside the electrode will not interact with the air; calcium fluoride can also increase the basicity of the cladding metal. The first core layer and the second core layer are clad. The first core layer and the second core layer match the high basicity environment formed by calcium fluoride. The P, S, O, and H contents in the cladding layer obtained are low, and the organization is a high-carbon martensite base plus dispersed and evenly distributed carbon, nitrides and a small amount of ferrite (such as Figure 3 shown), by Figure 3 It can be seen that the microstructure has fine and uniform grains, small diameter and few inclusions, so the cladding layer has high toughness and good high-temperature stability; titanium powder and magnesium oxide have the function of adjusting the molten droplet transition morphology, welding spatter and weld bead formation; calcium carbonate is appropriately added to the outer coating, which increases the oxidizing property of the arc atmosphere in the arc column area;
[0028] At this time, the following reaction can be carried out in the arc column: CO2+H2→CO+H2O
[0029] 2H2+O2→2H2O
[0030] This reduces the hydrogen partial pressure in the arc column region and can effectively control the generation of hydrogen pores.
[0031] The coating layer is set on the outside of the steel strip, and the coating layer is easy to crack; the cracks in the coating layer include longitudinal cracks (along the axial direction), transverse cracks and tortoise cracks, etc. When the coating layer cracks, the coating will fall off during welding, resulting in welding defects such as pores in the weld, affecting the intrinsic performance of the roll welding; Figure 2 As shown, an aluminum mesh is arranged in a ring shape on the outside of the steel strip and the inside of the coating layer. The mesh size of the aluminum mesh is 20-80 meshes, and the thickness of the aluminum mesh is 0.2mm-0.8mm. The aluminum mesh is arranged in the middle of the coating layer to play a fixing role. At the same time, after the aluminum mesh is melted, the aluminum metal acts as a reducing agent to reduce the residual amount of oxygen in the cladding metal and improve the quality of the cladding.
[0032] Example 1
[0033] The steel strip is low-carbon steel HS1 steel strip, the thickness of the steel strip is 0.5mm, and the diameter of the cylinder surrounded by the steel strip is 3.2mm; the composition (mass percentage) of the first core layer and the second core layer are both high-carbon ferrochrome 30%; molybdenum powder 8%; ferrovanadium 3%; niobium powder 12%; manganese powder 6%, aluminum powder 4%; iron powder balance; the sum of each component is 100%;
[0034] The volume ratio of the first drug core layer to the second drug core layer is 2:3; the particle size of the first drug core layer is 180 mesh, and the particle size of the second drug core layer is 140 mesh.
[0035] Example 2
[0036] The steel strip is low-carbon steel HS1 steel strip, the thickness of the steel strip is 0.5mm, and the diameter of the cylinder surrounded by the steel strip is 3.2mm; the composition (mass percentage) of the first core layer and the second core layer are both high-carbon ferrochrome 30%; molybdenum powder 8%; ferrovanadium 3%; niobium powder 12%; manganese powder 6%, aluminum powder 4%; iron powder balance; the sum of each component is 100%;
[0037] The volume ratio of the first drug core layer to the second drug core layer is 2:3; the particle size of the first drug core layer is 180 mesh, and the particle size of the second drug core layer is 140 mesh;
[0038] A coating layer is arranged on the outer side of the steel strip, and the coating layer is composed of the following raw materials in percentage by mass: 35% calcium fluoride, 40% titanium powder, 20% magnesium oxide, and 5% calcium carbonate.
[0039] Example 3
[0040] The steel strip is low-carbon steel HS1 steel strip, the thickness of the steel strip is 0.5mm, and the diameter of the cylinder surrounded by the steel strip is 3.2mm; the composition (mass percentage) of the first core layer and the second core layer are both high-carbon ferrochrome 30%; molybdenum powder 8%; ferrovanadium 3%; niobium powder 12%; manganese powder 6%; aluminum powder 4%; iron powder balance;
[0041] The volume ratio of the first drug core layer to the second drug core layer is 2:3; the particle size of the first drug core layer is 180 mesh, and the particle size of the second drug core layer is 140 mesh;
[0042] A coating layer is provided on the outside of the steel strip, and the coating layer is composed of the following raw materials in percentage by mass: 35% calcium fluoride, 40% titanium powder, 20% magnesium oxide, and 5% calcium carbonate;
[0043] An aluminum mesh is arranged in a ring shape on the outside of the steel belt and the inside of the coating layer. The mesh size of the aluminum mesh is 50 meshes and the thickness of the aluminum mesh is 0.5 mm.
[0044] Comparative Example 1
[0045] The steel strip is low-carbon steel HS1 steel strip, the thickness of the steel strip is 0.5mm, and the diameter of the cylinder surrounded by the steel strip is 3.2mm; the steel strip is filled with a core layer (mass percentage), high-carbon ferrochrome 30%; molybdenum powder 8%; ferrovanadium 3%; niobium powder 12%; manganese powder 6%, aluminum powder 4%; iron powder balance; the sum of each component is 100%;
[0046] The particle size of the drug core layer is 180 mesh.
[0047] Comparative Example 2
[0048] The steel strip is low-carbon steel HS1 steel strip, the thickness of the steel strip is 0.5mm, and the diameter of the cylinder surrounded by the steel strip is 3.2mm; the steel strip is filled with a core layer (mass percentage), high-carbon ferrochrome 30%; molybdenum powder 8%; ferrovanadium 3%; niobium powder 12%; manganese powder 6%, aluminum powder 4%; iron powder balance; the sum of each component is 100%;
[0049] The particle size of the drug core layer is 240 mesh.
[0050] Comparative Example 3
[0051] The steel strip is low-carbon steel HS1 steel strip, the thickness of the steel strip is 0.5mm, and the diameter of the cylinder surrounded by the steel strip is 3.2mm; the steel strip is filled with a single core layer component (mass percentage), high-carbon ferrochrome 30%; molybdenum powder 8%; ferrovanadium 3%; niobium powder 12%; manganese powder 6%, aluminum powder 4%; iron powder balance; the sum of each component is 100%;
[0052] The particle size of the drug core layer is 140 mesh.
[0053] Comparative Example 4
[0054] The steel strip is low-carbon steel HS1 steel strip, the thickness of the steel strip is 0.5mm, and the diameter of the cylinder surrounded by the steel strip is 3.2mm; the steel strip is filled with a single core layer component (mass percentage), high-carbon ferrochrome 30%; molybdenum powder 8%; ferrovanadium 3%; niobium powder 12%; manganese powder 6%, aluminum powder 4%; iron powder balance; the sum of each component is 100%;
[0055] The particle size of the drug core layer is 60 mesh.
[0056] The evaluation results of the embodiments and comparative examples are shown in Table 1.
[0057] Table 1 Evaluation results of welding rods of embodiments and comparative examples
[0058]
[0059] It can be seen from Examples 1, 2, 3 and Comparative Examples 1, 2, 3, 4 that:
[0060] When welding, smaller particles will form finer grains, which will increase the hardness of the weld metal, but the toughness of the welding material will decrease; the core layer of the smaller particles surrounds the core layer of the larger particles, and the core layer of the smaller particles combines with the roller to be repaired to increase the bonding force, and the core layer of the smaller particles wraps the core layer of the larger particles to form a welding material with both high hardness and high toughness; an aluminum mesh is set in a ring on the inner side of the skin layer to avoid cracking of the skin layer to a certain extent.
[0061] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. The protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A flux-cored electrode for surfacing repair, characterized in that: It includes a steel strip and a first core layer and a second core layer wrapped inside the steel strip. The first core layer and the second core layer have the same composition, and the first core layer and the second core layer are composed of the following raw materials in percentage by mass: 25%-35% high carbon ferrochrome; 5%-10% molybdenum powder; 1%-5% ferrovanadium; 9%-15% niobium powder; 5%-7% manganese powder, 3%-4% aluminum powder; the remainder is iron powder, and the sum of each component is 100%; The particle size of the first drug core layer is greater than the particle size of the second drug core layer.
2. A flux-cored electrode for cladding repair according to claim 1, characterized in that: The steel belt is made of low-carbon steel HS1 steel belt, the thickness of the steel belt is 0.3-0.8 mm, and the diameter of the cylinder surrounded by the steel belt is 2.8 mm-4.0 mm.
3. A flux-cored electrode for cladding repair according to claim 1, characterized in that: The volume ratio of the first drug core layer to the second drug core layer is 2:2.5-3.5; the particle size of the first drug core layer is 160 mesh-200 mesh, and the particle size of the second drug core layer is 120 mesh-160 mesh.
4. A flux-cored electrode for surfacing repair according to claim 3, characterized in that: The volume ratio of the first drug core layer to the second drug core layer is 2:3; the particle size of the first drug core layer is 180 mesh, and the particle size of the second drug core layer is 140 mesh.
5. A flux-cored electrode for cladding repair according to claim 1, characterized in that: A coating layer is arranged on the outer side of the steel strip, and the coating layer is composed of the following raw materials in the following mass percentages: 30% to 40% calcium fluoride, 35% to 45% titanium powder, 15% to 25% magnesium oxide, and 4% to 6% calcium carbonate, and the sum of the components is 100%.
6. A flux-cored electrode for cladding repair according to claim 5, characterized in that: An aluminum mesh is annularly arranged on the outer side of the steel strip and the inner side of the coating layer.
7. A flux-cored electrode for cladding repair according to claim 6, characterized in that: The mesh size of the aluminum mesh is 20-80 meshes, and the thickness of the aluminum mesh is 0.2mm-0.8mm.
8. A flux-cored electrode for cladding repair according to claim 5, characterized in that: The drug skin layer is composed of the following raw materials in percentage by mass: 35% calcium fluoride, 40% titanium powder, 20% magnesium oxide and 5% calcium carbonate.