Carbon dioxide gas shielded solid welding wire steel wire rod capable of controlling splashing

By designing carbon dioxide gas shielded solid core welding wire steel wire rod, controlling the content of key elements and the addition of alloy elements, combined with strict preparation processes, the problem of welding spatter is solved, high-quality and efficient welding results are achieved, and the spatter rate and cost are reduced. , and improve welding safety.

CN118720516APending Publication Date: 2024-10-01BAOTOU IRON & STEEL (GROUP) CO LTD

Patent Information

Application Number
CN202410978908.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The spatter phenomenon during the welding process is serious, affecting the welding quality and efficiency, increasing costs, and there are risks of fire and explosion. The generation of spatter needs to be effectively controlled.

Method used

Design a carbon dioxide gas shielded solid core welding wire steel wire rod with controlled carbon content of 0.06-0.08%, silicon content of 0.35-0.45%, manganese content of 1.35-1.45%, phosphorus and sulfur content ≤0.020%, and aluminum and calcium content are strictly controlled, Ni, Cu, Cr, Ti alloy elements are added, and the low spatter welding wire steel wire rod preparation process includes molten iron desulfurization, converter, refining, continuous casting and rolling processes to ensure the cleanliness and reasonableness of the steel distribution of chemical components.

Benefits of technology

Significantly reduce welding spatter rate, improve welding quality and efficiency, reduce material costs, and improve welding environment and safety, reaching 550MPa weather resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720516A_ABST
    Figure CN118720516A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon dioxide gas shielded solid welding wire steel wire rod capable of controlling splashing. The carbon dioxide gas shielded solid welding wire steel wire rod comprises the following steps: designing the carbon content to be 0.06-0.08%; the silicon content is controlled to be 0.35 to 0.45 percent, and the manganese content is controlled to be 1.35 to 1.45 percent; phosphorus content and sulfur content are controlled to be less than or equal to 0.020%; al is controlled to be less than or equal to 0.01%, and Ca is controlled to be Ni alloy elements, Cu alloy elements and Cr alloy elements with different contents are added into the steel, and the adding ranges are 0.35%-0.45%, 0.25%-0.35% and 0.30%-0.40% respectively; ti is an element capable of obviously inhibiting welding spatter, so that a proper amount of titanium is added into the steel, and the adding amount is 0.02-0.05%; the oxygen content in the steel is less than or equal to 0.003%, and the nitrogen content is less than or equal to 0.005%. The invention further discloses a preparation method. The purpose of the invention is to achieve a strong level of welding, smooth drawing and reduced spatter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of smelting and rolling technology, and in particular relates to a carbon dioxide gas-protected solid welding wire steel wire rod for controlling splashing. Background Art

[0002] Spatter refers to the phenomenon that molten metal particles or slag fly around during welding. These spattered metal particles may interfere with the molten pool, resulting in reduced weld quality, such as defects such as slag inclusions and pores. The presence of spatter will also reduce welding productivity, especially when using large parameter welding such as CO2 gas shielded welding, spatter is more serious, and the spatter rate can reach more than 20%, seriously affecting welding efficiency. In addition, spatter will increase welding costs, and the metal spatter that falls on the surface of the welded workpiece needs to be polished and removed, which increases additional polishing costs.

[0003] Welding spatter will also reduce the welding efficiency of the welding wire, so that more welding wire is needed to complete the welding work, which increases the material cost. There is also a potential risk of fire and explosion. The temperature of welding spatter is very high. When it splashes on combustibles, it may cause a fire; when it comes into contact with explosive gases, it may cause an explosion. The power cord of the electric welding machine is often dragged and worn during operation, which can easily cause line damage and short circuits to cause fires in surrounding combustibles. In summary, the hazards of welding spatter cannot be ignored. It not only affects the welding quality and efficiency, but also affects the welding environment and safety, increases welding costs, and has potential fire and explosion risks. Appropriate measures should be taken to reduce and control the generation of spatter during the welding process. Therefore, a carbon dioxide gas shielded solid welding wire steel wire rod with controlled spatter is proposed. Summary of the invention

[0004] The purpose of the present invention is to provide a carbon dioxide gas-shielded solid welding wire steel wire rod with controlled spatter.

[0005] If the carbon content of the welding wire is too high, it will cause large spatter and produce pores due to the intense oxidation-reduction reaction during welding. Therefore, the carbon content of the welding wire should be low, and the carbon content should be at the lower limit. It is usually required to C <0.11%. Silicon is the most commonly used deoxidizing element in welding wire steel. It can prevent iron from combining with oxygen and can reduce FeO in the molten pool. However, when silicon is used alone for deoxidation, the SiO2 generated has a high melting point (about 1710℃), and the particles of the product are small, making it difficult to float out of the molten pool, which can easily cause slag inclusions in the weld metal. The role of manganese in steel is similar to that of silicon, but its deoxidation ability is slightly worse than that of silicon. When manganese is used alone for deoxidation, the density of MnO generated is relatively large (15.11g / cm 3) and it is not easy to float out of the molten pool. In addition to the deoxidation effect, manganese contained in the welding wire can also combine with sulfur to form manganese sulfide (MnS), which is removed (desulfurization), so the tendency of thermal cracks caused by sulfur can be reduced. Since it is difficult to remove the deoxidation products when using silicon and manganese for deoxidation alone. Therefore, silicon and manganese are often used for combined deoxidation to make the generated SiO2 and MnO compound into silicate (MnO·SiO2). MnO·SiO2 has a low melting point (about 1270℃) and a low density (about 3.6g / cm 3 ), it can condense into large pieces of slag in the molten pool and float out, achieving a good deoxidation effect. Manganese is also an important alloying element in steel and an important hardenability element. It has a great influence on the toughness of the weld metal. When the Mn content is less than 0.5%, the toughness of the weld metal is very high; when the Mn content is greater than 3%, it is very brittle; when the Mn content is 0.6-1.8%, the weld metal has higher strength and toughness. It is advisable to control the manganese content of welding wire steel at 1.40%-1.50%. If the P and S content of the welding wire is too high, it will also affect spatter. If the phosphorus content is too high, larger and higher-level inclusions will be formed, resulting in the inability of the current to completely melt the inclusions during welding and produce spatter. It is usually required that ω P<0.020%. Sulfur often exists in the form of iron sulfide in steel and is distributed in a network at the grain boundaries, thus significantly reducing the toughness of the steel. The eutectic temperature of iron plus iron sulfide is relatively low (985°C). Therefore, during hot working, since the processing start temperature is generally 1150-1200°C, the iron and iron sulfide eutectic has melted, resulting in cracking during processing. This phenomenon is the so-called "hot brittleness of sulfur". Too high sulfur content will increase the tendency of hot cracks in the weld and affect the welding quality. The sulfur content of welding wire steel should be controlled at 0.011% to 0.018%. When aluminum is used for deoxidation, the melting point of the generated Al2O3 is very high and it exists in the molten pool in a solid state, which is easy to cause slag inclusion in the weld. At the same time, aluminum-containing welding wire is prone to spattering, and too high aluminum content will also reduce the ability of the weld metal to resist hot cracks. Therefore, the aluminum content in the welding wire must be strictly controlled. The deoxidation method of welding steel adopts aluminum deoxidation or a small amount of aluminum in the raw and auxiliary materials. The Al2O3 generated has a high melting point and exists in the molten pool in a solid state, which is easy to cause weld slag. At the same time, it is also easy to cause spatter. Excessive aluminum content will also reduce the ability of weld metal to resist thermal cracking. Therefore, the aluminum content of general welding steel must be strictly controlled. According to the survey, the Al content in domestic welding wire steel is basically controlled below 0.01%. The calcium element of welding wire steel increases. After calcium oxidation, before the molten droplet falls off, the surface is enriched with oxides and oxygen ions. Elements such as K and Na are surface active elements that can effectively reduce the surface tension of the molten droplet, while alkaline oxides such as CaO, MgO, and A12O3 will increase the surface tension. At the same time, these alkaline oxides that can increase the surface tension of the molten droplet have high aggregation on the surface of the molten droplet and are easy to gather at the tip of the bottom of the molten droplet. Because the arc has the characteristics of oxide affinity, the force area of ​​the molten droplet is reduced and the force is uneven, which makes the molten droplet unstable and prone to spatter. It is advisable to control the calcium content of welding wire steel to ≤0.0015%. Titanium is also a strong deoxidizing element, and can also be combined with nitride to synthesize TiN to play a nitrogen fixing role, improving the ability of the weld metal to resist nitrogen porosity. If the content of Ti and B (boron) in the weld structure is appropriate, the weld structure can be refined. The iron oxide scale pressed into the surface of the welding wire will make the stability of the welding wire worse, and the uneven feeding of the welding wire is also one of the reasons for the high spatter rate. In summary, it can be seen that the main elements that affect the spatter of gas shielded welding wire steel are C, Ca, Al, P, and S content. Si, Ti, K, Na, etc. are all elements that can significantly inhibit spatter.

[0006] The cleanliness of steel is an indicator of the amount of harmful components in the steel composition, especially the number, size, shape and distribution of non-metallic inclusions. These inclusions may become the source of spatter during welding.

[0007] Inclusions such as Al2O3 may react with other elements in steel to produce gas at high welding temperatures. If these gases cannot be discharged in time, bubbles will form in the molten pool, and the rupture of the bubbles will cause spatter. Large macro inclusions are the most harmful to the mechanical properties of steel, and their size distribution has an important influence on welding spatter. It is reported that a typical low-carbon aluminum-killed steel may contain millions of inclusions, among which large inclusions may be small in number but the overall volume fraction may be large. Large inclusions are more likely to cause fluctuations and instability in the molten pool during welding, thereby increasing the generation of spatter. The cleanliness of steel not only affects welding spatter, but also directly affects the welding quality. Steel with high cleanliness is easier to obtain high-quality welds during welding, reducing the generation of defects such as slag inclusions and pores. The reduction of welding spatter also helps to improve welding efficiency, reduce welding costs, and improve welding environment and safety. In order to reduce welding spatter, it is necessary to control the cleanliness of steel. This includes reducing the content of non-metallic oxide inclusions in steel and controlling their morphology, chemical composition and size distribution, while reducing the content of impurity elements (such as S, P, H, N, etc.) and trace elements in steel. Strictly cleaning the steel before welding to remove surface oil, rust and other pollutants can also effectively reduce the generation of welding spatter.

[0008] In summary, the cleanliness of steel has an important influence on welding spatter. By controlling the cleanliness of steel and taking appropriate welding process measures, the generation of welding spatter can be effectively reduced and the welding quality and efficiency can be improved.

[0009] The iron oxide scale pressed into the base wire rod will also affect the spatter of welding. The iron oxide scale press-in refers to the quality defect caused by the iron oxide scale being accidentally pressed into the steel surface during the rolling process. At present, the iron oxide scale of welding steel is mostly removed by mechanical peeling. It is difficult to remove the pressed iron oxide scale in this way, and it will remain on the surface of the finished drawn welding wire steel. The iron oxide scale becomes iron oxide, which will also cause serious spatter during welding.

[0010] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0011] The present invention discloses a carbon dioxide gas shielded solid welding wire steel wire rod for controlling spatter, comprising:

[0012] The designed carbon content is 0.06-0.08%;

[0013] Control the silicon content to 0.35-0.45% and the manganese content to 1.35-1.45%;

[0014] Control phosphorus content and sulfur content ≤ 0.020%;

[0015] Control Al≤0.01%, Ca≤0.001%;

[0016] Different contents of Ni, Cu and Cr alloy elements are added to the steel, with the addition ranges of 0.35-0.45%, 0.25-0.35% and 0.30-0.40% respectively; Ti is an element that can obviously inhibit welding spatter, so an appropriate amount of titanium is added to the steel, with the addition amount of 0.02-0.05%;

[0017] Ensure that the oxygen content in the steel is ≤0.003% and the nitrogen content is ≤0.005%.

[0018] Furthermore, the manganese content of the welding wire steel is controlled at 1.40% to 1.42%.

[0019] Furthermore, the sulfur content of the welding wire steel is controlled at 0.011% to 0.018%.

[0020] Furthermore, Al is controlled to be ≤ 0.005%.

[0021] Furthermore, the titanium content is controlled within the range of 0.02 to 0.05%.

[0022] The specific preparation method comprises:

[0023] The production process of low spatter welding wire steel wire rod is as follows: hot metal desulfurization - converter - refining - continuous casting - rolling.

[0024] After desulfurization treatment, the sulfur content of the hot metal entering the furnace is ≤0.020%. The weight of the hot metal must be accurately controlled within a certain range, requiring 94 to 95 tons. The amount of scrap steel loaded into each furnace is controlled at 11 tons, and the final amount of the converter is controlled at 105 to 106 tons. The carbon content of the converter is controlled to 0.08% to 0.12%. The steel is blown once, and the second blow is not allowed. The tapping temperature is controlled to be no less than 1610℃, and the blow time is no more than 1.5 minutes. 200kg of dolomite thick slag is added to each furnace before tapping. The amount of lime used is increased or decreased according to the sulfur content of the steel, and the amount of refined lime used is low-splash welding wire steel wire rod preparation process: hot metal desulfurization-converter-refining-continuous casting-rolling. Control 2kg-4kg / t, and use fluorite balls for slag material. Refining dust removal uses a micro-positive pressure to isolate the inhalation of nitrogen content. The Al content is controlled during the refining process. Since Al is a nitrogen-fixing element, the precipitated AlN has a serious impact on work hardening, so the Al content is controlled to be ≤0.005%. The production rhythm is controlled well during the refining process to avoid long-term power supply and soft blowing operations. When pouring, the argon gas is used to replace the middle bag, and the time must be ≥3min to ensure that the middle bag is full of argon and there is no residual air. The argon blowing time for each furnace must be recorded. The long water nozzle of each steel ladle in each furnace uses an asbestos bowl and argon is blown, and the T-shaped steel liquid does not emit carbon flowers. When pouring, each water nozzle must also be replaced with air, and when changing the water nozzle, argon gas must also be purged to ensure that there is no residual air.

[0025] The rolling process parameters are as follows:

[0026] Rolling temperature: 1040±20℃.

[0027] Finishing rolling entrance temperature: 850±20℃, limit control. Wire laying temperature: 830℃±10℃.

[0028] Insulation cover: Fully closed includes the first two groups, a total of 20.

[0029] Fan: All off.

[0030] Starting roller speed: 0.10m / s.

[0031] Compared with the prior art, the beneficial technical effects of the present invention are:

[0032] The invention provides a 550MPa weather-resistant carbon dioxide gas shielded welding wire rod for reducing welding spatter, which achieves the purpose of welding strength level, smooth drawing and reduced spatter. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the oxidized iron scale of the base material wire rod. DETAILED DESCRIPTION

[0034] The present invention will be further described below in conjunction with the embodiments.

[0035] In order to further clarify, a 550MPa weather-resistant carbon dioxide gas shielded welding wire rod that reduces welding spatter is used as an example. In order to achieve the strong level of welding, smooth drawing and reduce spatter, the carbon content is designed to be 0.06-0.08%; silicon and manganese are alloying elements that inhibit welding spatter, but high silicon is easy to form sticky iron oxide scale that is difficult to remove. Therefore, in order to ensure strength and remove iron oxide scale at the same time, the silicon content is controlled to be 0.35-0.45%, and the manganese content is controlled to be 1.35-1.45%; excessive phosphorus content will also form larger and higher-level inclusions, resulting in the current being unable to completely melt the inclusions during welding and causing spatter. Sulfur often exists in the form of iron sulfide in steel and is distributed in a network at the grain boundaries, thus significantly reducing the toughness of the steel. Therefore, the phosphorus content and sulfur content are controlled to be ≤0.020%; the aluminum and calcium content in the steel must be controlled, and control measures are proposed requiring Al≤0.005%, Ca≤0.001%; ​​in order to ensure that the atmospheric corrosion resistance I factor after welding is greater than 6.0, different contents of Ni, Cu, and Cr alloy elements are added to the steel, and the addition ranges are 0.35-0.45%, 0.25-0.35%, and 0.30-0.40%, respectively; Ti is an element that can obviously inhibit welding spatter, so an appropriate amount of titanium is added to the steel, and the addition amount is 0.02-0.05%; in order to reduce welding spatter, the cleanliness of the steel needs to be controlled. This includes reducing the content of non-metallic oxide inclusions in steel and controlling their morphology, chemical composition and size distribution, while reducing the content of impurity elements and trace elements in steel, ensuring that the oxygen content in the steel is ≤0.003% and the nitrogen content is ≤0.005%; the thickness of the oxide scale of the base material wire rod obtained by rolling should be uniform, without obvious pressed oxide scale, as shown in the following examples: Figure 1 The above mentioned contents are all in mass percentage.

[0036] Table 1 Specific ingredients of each embodiment 1

[0037]

[0038] Table 2 Mechanical properties of each embodiment 1

[0039]

[0040] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A carbon dioxide gas shielded solid welding wire steel wire rod with controlled spatter, characterized in that: include: The designed carbon content is 0.06-0.08%; Control the silicon content to 0.35-0.45% and the manganese content to 1.35-1.45%; Control phosphorus content and sulfur content ≤ 0.020%; Control Al≤0.01%, Ca≤0.001%; Different contents of Ni, Cu and Cr alloy elements are added to the steel, with the addition ranges of 0.35-0.45%, 0.25-0.35% and 0.30-0.40% respectively; Ti is an element that can obviously inhibit welding spatter, so an appropriate amount of titanium is added to the steel, with the addition amount of 0.02-0.05%; Ensure that the oxygen content in the steel is ≤0.003% and the nitrogen content is ≤0.005%.

2. The carbon dioxide gas shielded solid welding wire steel wire rod with controlled spatter according to claim 1, characterized in that: The manganese content of welding wire steel is controlled at 1.40% to 1.42%.

3. The carbon dioxide gas shielded solid welding wire steel wire rod with controlled spatter according to claim 2, characterized in that: The sulfur content of welding wire steel is controlled at 0.011% to 0.018%.

4. The carbon dioxide gas shielded solid welding wire steel wire rod with controlled spatter according to claim 2, characterized in that: Control Al≤0.005%, and control titanium at 0.02~0.05%.

5. The method for preparing the carbon dioxide gas shielded solid welding wire steel wire rod with controlled spatter according to claim 1, characterized in that: The preparation process includes: molten iron desulfurization - converter - refining - continuous casting - rolling.

Citation Information

Patent Citations

  • High-quality welding wire steel wire rod and production method thereof

    CN108393614A

  • Low-spatter-rate ER50-6 gas-protection solid welding wire

    CN109514127A

  • Method of improving quality of welding wire steel casting blank

    CN111716037A

  • High-weather-resistance low-splashing wire rod for gas shielded welding wire and welding wire

    CN113681198A

  • Production method of annealing-free weather-resistant wire rod for vehicle welding wire steel

    CN116497263A

Cited By

  • Wire rod for low-aluminum low-calcium sulfur-control gas shield welding wire and production method of wire rod

    CN120644860A