Processing technology and processing equipment of ceramic femoral head
Through the grinding and mechanical processing of ceramic blank balls, combined with a V-groove grinder, the problem of low processing efficiency of ceramic femoral heads is solved, efficient and low-cost production of ceramic femoral heads is achieved, and the cost of artificial joint replacement is reduced. .
Patent Information
- Application Number
- CN202410754857.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-01-31
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The low processing efficiency of ceramic femoral heads leads to high costs, which hinders the development of artificial joint replacement.
Ceramic rough balls made of zirconia reinforced alumina, silicon nitride, alumina, silicon carbide and other materials are used for grinding and mechanical processing, including rough grinding, fine grinding, fine grinding and fine polishing, using abrasives such as diamond and boron carbide And water-based or oil-based grinding fluid, combined with V-groove grinder for grinding, gradually improve the accuracy and surface finish of ceramic balls.
The processing efficiency of the ceramic femoral head is improved, the preparation cost is reduced, and the efficient and low-cost production of the ceramic femoral head is achieved.
Smart Images

Figure CN118720863A_ABST
Abstract
Description
[0001] This application claims the priority of Chinese patent application 2024101390588 filed on January 31, 2024, and incorporates the entire contents of this patent application by introduction. Technical Field
[0002] The invention relates to the technical field of ceramic femoral head processing, and in particular to a processing technology and processing equipment for a ceramic femoral head. Background Art
[0003] Artificial joint replacement is a surgical method that uses surgical methods to replace the joint surface damaged by disease or injury with an artificial joint to remove the lesion, eliminate pain, and restore joint movement and original function. Ceramic femoral head is a medical device product made of inorganic non-metallic materials, more precisely advanced structural ceramics, for implantation in the human body.
[0004] Clinical applications have shown that ceramic femoral heads have been widely welcomed by doctors and patients due to their good biocompatibility, extremely high wear resistance and corrosion resistance, and will surely become the basis for the promotion and application of ceramic artificial joint replacement in the future. The ceramic femoral head used for human hip joint prosthesis is usually made of ceramic raw material powder through compression molding, high temperature sintering to obtain a blank body, and then mechanically processed into a ceramic femoral head finished product with the required size and surface finish (roughness). Unlike the plastic processing of metal materials, ceramic materials are brittle processing, so the processing efficiency of ceramics is very low. The ceramic femoral head mechanical processing in the prior art first presses the ceramic raw material powder into a partially spherical body with holes, and then sintered at high temperature to obtain a partially spherical blank body with holes. The partially spherical blank body with holes is rounded and polished, and the holes and tapers are ground and chamfered to obtain the ceramic femoral head finished product. However, the machines required for the above-mentioned preparation process are relatively expensive and the processing efficiency is low, so that the cost of the prepared ceramic femoral head is high, so the cost of artificial joint replacement is increased, which becomes one of the obstacles to the development of artificial joint replacement. While ensuring the processing quality of ceramic femoral heads, improving the processing efficiency of ceramic femoral heads is the key to their application in the medical field.
[0005] Therefore, it is urgent to develop a processing technology and processing equipment for ceramic femoral head to solve the above problems. Summary of the invention
[0006] The purpose of the present invention is to provide a processing technology and processing equipment for a ceramic femoral head, which solves the problem of high cost caused by low processing efficiency of the ceramic femoral head in the prior art.
[0007] To achieve the above object, in a first aspect, the present invention provides a processing technology for a ceramic femoral head, comprising the following steps:
[0008] S0: providing a ceramic blank ball, wherein the material of the ceramic blank ball includes at least one of zirconium oxide reinforced aluminum oxide, silicon nitride, aluminum oxide, zirconium oxide and silicon carbide;
[0009] S1: grinding the ceramic rough ball to obtain a ceramic ball;
[0010] S2: Mechanically processing the ceramic ball to obtain the ceramic femoral head.
[0011] The beneficial effect of the processing technology of the ceramic femoral head of the present invention is that the ceramic blank ball is first ground to obtain a ceramic ball, and then the ceramic ball is mechanically processed to obtain a ceramic femoral head. The processing technology of the present invention is simple and efficient, which reduces the preparation cost of the ceramic femoral head.
[0012] Optionally, the abrasive for the grinding treatment is at least one of diamond, boron carbide, cubic boron nitride and silicon carbide, the grinding liquid for the grinding treatment is any one of water-based grinding liquid and oil-based grinding liquid, the grinding pressure for the grinding treatment is 2-5MPa, and the temperature for the grinding treatment is 0-50°C.
[0013] Optionally, the grinding process includes coarse grinding, fine grinding, lapping and polishing in sequence;
[0014] The rough grinding process includes: placing the ceramic blank ball into a first processing device for rough grinding to obtain a rough ground ceramic blank ball;
[0015] The fine grinding process comprises: placing the coarsely ground ceramic blank ball into a second processing device for fine grinding to obtain a finely ground ceramic blank ball;
[0016] The lapping process comprises: placing the finely ground ceramic blank ball into a third processing device for lapping to obtain a lapping ceramic blank ball;
[0017] The fine polishing treatment includes: placing the finely ground ceramic blank ball into a fourth processing device for fine polishing to obtain the ceramic ball.
[0018] Optionally, the step of placing the ceramic blank ball into a first processing device for rough grinding to obtain a rough ground ceramic blank ball specifically comprises the following steps:
[0019] placing the ceramic blank ball into the first processing equipment;
[0020] placing a coarse abrasive in the first processing equipment;
[0021] The rotation speed of the first processing equipment is set to 30-50 r / min to rough-grind the ceramic blank ball to obtain the rough-grinded ceramic blank ball.
[0022] Optionally, the step of placing the coarsely ground ceramic blank ball into a second processing device for fine grinding to obtain a finely ground ceramic blank ball specifically comprises the following steps:
[0023] placing the roughly ground ceramic blank ball into the second processing equipment;
[0024] placing fine abrasive in the second processing equipment;
[0025] The rotation speed of the second processing equipment is set to 20-40 r / min to finely grind the coarsely ground ceramic blank ball to obtain the finely ground ceramic blank ball.
[0026] Optionally, the step of placing the finely ground ceramic blank ball into a third processing device for fine grinding to obtain a finely ground ceramic blank ball specifically comprises the following steps:
[0027] placing the finely ground ceramic rough ball into the third processing equipment;
[0028] placing finely ground material into the third processing equipment;
[0029] The rotation speed of the third processing equipment is set to 20-40 r / min to grind the fine-ground ceramic blank ball to obtain the grinded ceramic blank ball.
[0030] Optionally, the step of placing the finely ground ceramic rough ball into a fourth processing device for fine polishing to obtain the ceramic ball specifically comprises the following steps:
[0031] placing the finely ground ceramic blank ball into the fourth processing equipment;
[0032] placing a polishing agent in the fourth processing equipment;
[0033] The rotation speed of the fourth processing equipment is set to 20-40 r / min to perform fine polishing on the finely ground ceramic blank ball to obtain the ceramic ball.
[0034] Optionally, coarse abrasive is added to the first processing equipment, the mesh size of the coarse abrasive is 60-600 mesh, fine abrasive is added to the second processing equipment, the particle size of the fine abrasive is 3-5 microns, and fine abrasive is added to the third processing equipment, the particle size of the fine abrasive is 0.8-1.2 microns.
[0035] Optionally, the coarse abrasive includes diamond with a mesh size of 60-600 meshes, the fine abrasive includes diamond with a particle size of 3-5 microns, and the fine abrasive includes diamond with a particle size of 0.8-1.2 microns.
[0036] Optionally, the removal rate of the ceramic blank ball in the rough grinding process is 5-10 microns / hour, the removal rate of the rough ground ceramic blank ball in the fine grinding process is 0.1-0.6 microns / hour, the removal rate of the fine ground ceramic blank ball in the fine grinding process is 0.1-0.6 microns / hour, and the removal rate of the fine ground ceramic blank ball in the fine polishing process is 0.1-0.3 microns / hour.
[0037] Optionally, the machining allowance of the ceramic blank ball is 30-50 microns, the machining allowance of the coarsely ground ceramic blank ball is 30-100 microns, the machining allowance of the finely ground ceramic blank ball is 5-30 microns, the machining allowance of the finely ground ceramic blank ball is 1-5 microns, and the diameter tolerance of the ceramic ball after fine polishing is -0.1-0.1 microns.
[0038] Optionally, the specific steps of mechanically processing the ceramic ball to obtain the ceramic femoral head include: grinding a plane on the ceramic ball, and sequentially performing hole grinding, grinding and chamfering on the plane to obtain the ceramic femoral head.
[0039] In a second aspect, the present invention provides a processing device for a ceramic femoral head, wherein the grinding process is performed in the processing device, and the processing device includes a base, a fixed disk, a rotating disk, a rotating shaft and a driving device, wherein the fixed disk is fixedly connected to the base, the rotating disk is fixedly connected to the rotating shaft, the rotating shaft rotates under the drive of the driving device and drives the rotating disk to rotate, and a plurality of V-shaped grooves are provided on a side of the rotating disk close to the fixed disk.
[0040] Optionally, the angle of the V-shaped groove is 70°-90°, the horizontal distance between the central axis of the V-shaped groove and the central axis of the fixed disk is less than 10°, and the horizontal distance between the central axis of the V-shaped groove and the central axis of the rotating disk is less than 10°. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a structural schematic diagram of a ceramic femoral head processing device according to an embodiment of the present invention;
[0042] Figure 2 This is a schematic structural diagram of a first powder ceramic rough ball according to an embodiment of the present invention;
[0043] Figure 3 Schematic diagram of the structure of the second powder pottery rough ball according to an embodiment of the present invention. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] The core of the invention of this patent is: the ceramic raw material powder is pressed into shape and sintered at high temperature to obtain a complete spherical blank, the complete spherical blank is rounded and polished, and then a flat surface is ground on the sphere, a hole is opened (also a grinding process), the hole taper is ground, and the chamfer is ground to obtain a ceramic femoral head, which solves the problem of high cost caused by low processing efficiency of ceramic femoral heads in the prior art.
[0046] An embodiment of the present invention provides a processing technology for a ceramic femoral head, comprising the following steps:
[0047] S0: providing a ceramic blank ball, wherein the material of the ceramic blank ball includes at least one of zirconium oxide reinforced aluminum oxide, silicon nitride, aluminum oxide, zirconium oxide and silicon carbide;
[0048] S1: grinding the ceramic rough ball to obtain a ceramic ball;
[0049] S2: Mechanically processing the ceramic ball to obtain the ceramic femoral head.
[0050] Specifically, the ceramic raw material powder is pressed into shape and sintered at high temperature to obtain a complete ceramic blank ball, the ceramic blank ball is first rounded and polished to obtain a ceramic ball, and then the surface, holes, hole tapers and chamfers are ground on the sphere of the ceramic ball to obtain a ceramic femoral head. The processing technology of the present invention is simple and efficient, which reduces the preparation cost of the ceramic femoral head.
[0051] Specifically, the ceramic blank ball includes at least one of zirconium oxide reinforced alumina, silicon nitride, aluminum oxide, zirconium oxide and silicon carbide. Among them, zirconium oxide reinforced alumina is a composite of 20%-30% zirconium oxide and 70%-80% aluminum oxide. The ceramic blank ball prepared by using zirconium oxide reinforced alumina material can be called a powder ceramic blank ball. The ceramic blank ball prepared by using silicon nitride material can be called a black ceramic blank ball. The ceramic blank ball prepared by using aluminum oxide material can be called a yellow ceramic blank ball.
[0052] In some embodiments of the present invention, the abrasive for the grinding treatment is at least one of diamond, boron carbide, cubic boron nitride and silicon carbide, the grinding liquid for the grinding treatment is any one of a water-based grinding liquid and an oil-based grinding liquid, the grinding pressure for the grinding treatment is 2-5MPa, and the temperature for the grinding treatment is 0-50°C.
[0053] In some embodiments of the present invention, the grinding process includes coarse grinding, fine grinding, lapping and polishing in sequence, and the specific steps include:
[0054] Rough grinding treatment: placing the ceramic blank ball into a first processing device, placing a coarse abrasive into the first processing device, and coarsely grinding the ceramic blank ball at a rotation speed of 30-50 r / min to obtain a coarsely ground ceramic blank ball;
[0055] Fine grinding treatment: placing the coarsely ground ceramic blank ball into a second processing device, placing fine abrasive in the second processing device, and fine grinding the coarsely ground ceramic blank ball at a rotation speed of 20-40 r / min by the second processing device to obtain a finely ground ceramic blank ball;
[0056] Lapping treatment: placing the finely ground ceramic blank ball into a third processing device, placing finely ground materials into the third processing device, and lapping the finely ground ceramic blank ball at a rotation speed of 20-40 r / min to obtain a lapping ceramic blank ball;
[0057] Fine polishing treatment: putting the finely ground ceramic blank ball into a fourth processing device, putting a polishing agent into the fourth processing device, and fine polishing the finely ground ceramic blank ball at a rotation speed of 20-40r / min to obtain a ceramic ball.
[0058] In some embodiments of the present invention, the polishing agent includes at least one of a rare earth polishing agent and a chromium trioxide polishing agent, and the polishing agent is not limited to the rare earth polishing agent and the chromium trioxide polishing agent.
[0059] In some embodiments of the present invention, the mesh size of the coarse abrasive is 60-600 mesh, the particle size of the fine abrasive is 3-5 microns, and the particle size of the fine abrasive is 0.8-1.2 microns.
[0060] In some embodiments of the present invention, the coarse abrasive includes diamond with a mesh size of 60-600 mesh, the fine abrasive includes diamond with a particle size of 3-5 microns, and the fine abrasive includes diamond with a particle size of 0.8-1.2 microns.
[0061] In some embodiments of the present invention, the removal rate of the ceramic blank ball in the rough grinding process is 5-10 microns / hour, the removal rate of the rough ground ceramic blank ball in the fine grinding process is 0.1-0.6 microns / hour, the removal rate of the fine ground ceramic blank ball in the fine grinding process is 0.1-0.6 microns / hour, and the removal rate of the fine ground ceramic blank ball in the fine polishing process is 0.1-0.3 microns / hour.
[0062] In some embodiments of the present invention, the machining allowance of the ceramic blank ball is 30-50 microns, the machining allowance of the coarsely ground ceramic blank ball is 30-100 microns, the machining allowance of the finely ground ceramic blank ball is 5-30 microns, the machining allowance of the finely ground ceramic blank ball is 1-5 microns, and the diameter tolerance of the ceramic ball after fine polishing is -0.1-0.1 microns.
[0063] In some embodiments of the present invention, the machining allowance of the ceramic rough ball refers to the thickness of the ceramic layer to be removed during the machining of the ceramic rough ball to obtain the machining surface required by the design by removing the excess ceramic on the surface to be machined on the ceramic rough ball through mechanical machining. In some more specific embodiments, 1 thread = 10 microns.
[0064] In some embodiments of the present invention, the specific steps of mechanically processing the ceramic ball to obtain the ceramic femoral head include: grinding a plane on the ceramic ball, and sequentially performing hole grinding, grinding and chamfering on the plane to obtain the ceramic femoral head.
[0065] An embodiment of the present invention provides a processing device for a ceramic femoral head, wherein the grinding process is performed in the processing device, and the processing device includes a base, a fixed disk, a rotating disk, a rotating shaft and a driving device. The fixed disk is fixedly connected to the base, and the rotating disk is fixedly connected to the rotating shaft. The rotating shaft rotates under the drive of the driving device and drives the rotating disk to rotate. A plurality of V-shaped grooves are provided on a side of the rotating disk close to the fixed disk.
[0066] In some embodiments of the present invention, an abrasive adding port is further provided on a side of the fixed disk away from the rotating disk.
[0067] In some embodiments of the present invention, the angle of the V-shaped groove is 70°-90°, the horizontal distance between the central axis of the V-shaped groove and the central axis of the fixed disk is less than 10°, and the horizontal distance between the central axis of the V-shaped groove and the central axis of the rotating disk is less than 10°.
[0068] Ceramic balls usually refer to silicon nitride balls, alumina balls, zirconia balls and silicon carbide balls, or a composite of these four materials, such as zirconia reinforced alumina ceramic balls; these ceramic balls have the characteristics of high hardness, high strength and wear resistance, so their machining difficulty is much greater than that of metals and engineering plastics.
[0069] After sintering, the dimensional accuracy and surface quality of ceramic balls are far from meeting the use requirements, and they need to be precisely ground. The ultimate goals of ceramic ball grinding are: (1) to achieve the requirements of dimensional accuracy, geometric shape accuracy and surface roughness of parts; (2) to eliminate surface defects.
[0070] Ceramics are hard and brittle materials, and material removal during machining is accomplished by brittle fracture. The indentation fracture model explains this process, which considers the interaction between abrasive particles and workpieces as a small-scale indentation phenomenon: in machining, each abrasive particle is equivalent to an indenter, and directly below the indenter is a plastic zone. Two main crack systems are formed from the plastic zone: central / radial cracks and transverse cracks. Central / radial cracks usually lead to a decrease in material strength, and transverse cracks extend laterally on a surface almost parallel to the workpiece surface. The deviation of cracks to the free surface leads to the fracture removal of materials (forming debris). Hardness represents the ability of ceramic materials to resist the indentation of abrasive particles into the material, and toughness represents the ability of ceramic materials to hinder crack extension. From the indentation fracture model, it can be seen that the fragmentation removal of ceramic materials is directly related to their hardness and toughness. The indentation fracture model is also suitable for explaining the beneficial effect of fine abrasive particles on the strength maintenance of ceramic materials. The normal force of a single abrasive particle is a function of the abrasive particle size, and it decreases significantly with the decrease of the abrasive particle size. It can be considered that the size of the central / radial crack caused by the abrasive particles decreases, and the ceramic material has higher strength at this time.
[0071] Due to the different mechanical properties of the four major engineering ceramics, the indentation morphologies exhibited under the same conditions are also different, so the processing efficiency exhibited in actual grinding processing is also different.
[0072] In the actual grinding process, an effective abrasive not only bears normal loads such as fixed-point indentation, but also bears tangential loads in the direction of movement. The tangential force will increase the normal tensile stress in the direction of movement of the contact point, which will promote the expansion of the central crack of the moving surface. The tangential force will also promote the expansion of transverse cracks in the direction of movement, accelerate the formation of debris, and remove materials.
[0073] In the actual grinding process, a large number of abrasive particles of various shapes and sizes randomly grind on the ball surface. In front of the movement of the abrasive particles, the ceramic ball material is quickly removed; below the abrasive particles, the force of each abrasive particle is different at each moment, resulting in a large difference in the size of the crushing zone. Generally, large abrasive particles produce greater stress, deeper crushing zone, and wider cracks, while small abrasive particles cause shallower crushing zone and finer cracks, which manifests as an uneven surface from a macroscopic perspective.
[0074] Some embodiments of the present invention refer to Figure 1, the processing equipment for batch processing of ceramic balls mainly adopts a concentric V-groove grinder, which includes a base 1, a fixed disk 2, a rotating disk 3, a rotating shaft 4 and a driving device 5. The fixed disk 2 is fixedly connected to the base 1, and the rotating disk 3 is fixedly connected to the rotating shaft 4. The rotating shaft 4 rotates under the drive of the driving device and drives the rotating disk 3 to rotate. A plurality of V-grooves 31 are opened on the side of the rotating disk 3 close to the fixed disk 2. The ceramic balls 6 are placed in the V-grooves 31, so the ceramic balls 6 are in a contact state between the rotating disk 3 and the fixed disk 2, and the optimal state is a three-arc contact state. The hardness of the fixed disk 2 and the rotating disk 3 is much lower than that of the ceramic ball 6, and the hardness of the abrasive is higher than that of the ceramic ball 6. Under the combined effect of the grinding pressure and the rotation of the fixed disk 2 and the rotating disk 3, part of the abrasive is squeezed and embedded in the contact surface of the fixed disk 2 and the rotating disk 3 with the ceramic ball 6, forming a very fine grinding tool. The rotating shaft 4 rotates under the drive of the driving device and drives the rotating disk 3 to rotate, and the ceramic ball 6 rolls in the V-shaped groove 31. On the one hand, the ceramic ball 6 revolves with the rotating disk 3, and on the other hand, the ceramic ball 6 continuously rotates. Therefore, the surface of the ceramic ball 6 and the contact surface of the fixed disk 2 and the rotating disk 3 produce relative sliding and rolling. At this time, the abrasive particles produce a grinding effect on the ceramic ball 6, including: using the abrasive particles to scrape the spherical surface of the ceramic ball to remove the excess; using the rolling effect of the abrasive particles to process the spherical surface of the ceramic ball; using the cutting edge of the abrasive particles to squeeze the ceramic ball, thereby completing the ceramic ball processing.
[0075] Some embodiments of the present invention refer to Figure 1 The fixed plate 2 is fixedly connected to the base through the connecting rod 7.
[0076] Some embodiments of the present invention refer to Figure 1 The angle of the V-shaped groove 31 is α, and the range of α is 70°-90°, preferably 90°.
[0077] In some embodiments of the present invention, the first processing equipment, the second processing equipment, the third processing equipment and the fourth processing equipment have the same structure, and the difference is that the diameter and material of the fixed disk and the rotating disk of the first processing equipment, the second processing equipment, the third processing equipment and the fourth processing equipment may be the same or different.
[0078] In some embodiments of the present invention, the fixed disk and the rotating disk are carriers for coating or embedding abrasives, so that the abrasives can play a cutting role, and are also grinding forming tools. The fixed disk and the rotating disk themselves are mutually corrected with the ceramic ball during the grinding process, and the geometric accuracy of the fixed disk and the rotating disk themselves is transferred to the workpiece to a certain extent, so the profiles of the fixed disk and the rotating disk are required to have high geometric accuracy. The main requirements for the fixed disk and the rotating disk are: the material hardness of the fixed disk and the rotating disk is generally lower than that of the ceramic ball material, and the hardness consistency is good, the structure is uniform and dense, without impurities, foreign matter, pores, cracks and other defects, and has a certain degree of abrasive embedding and impregnation; the fixed disk and the rotating disk have a reasonable structure, and have good rigidity, geometric accuracy retention and wear resistance.
[0079] In some embodiments of the present invention, the fixed disk and the rotating disk are cast iron disks, and the hardness is generally 140-220HB. The fixed disk is fixed, with a plane, the flatness of which is within 5 threads, and the fixed disk is also provided with an abrasive addition port, and the manufacturer of the fixed disk will process the abrasive addition port according to the purchase requirements; the rotating disk rotates with the rotating shaft, and a plurality of V-grooves are provided on the side of the rotating disk close to the fixed disk, the angle of the V-groove is 90°, and the groove width of the V-groove is determined according to the size of the ceramic ball. The groove width of the V-groove corresponding to the ceramic ball with a diameter of 28mm is 30mm, and the groove width of the V-groove corresponding to the ceramic ball with a diameter of 32mm is 34mm. The concentricity of the V-groove and the fixed disk is within 10 threads, and the concentricity of the V-groove and the rotating disk is within 10 threads. The diameters of the fixed disk and the rotating disk are not limited here. In some specific embodiments, the diameters of the fixed disk and the rotating disk range from 500 mm to 2800 mm.
[0080] In some embodiments of the present invention, during grinding processing, the number of the ceramic balls in the V-shaped groove should not be too large, and a certain gap should be ensured between each ceramic ball to facilitate the rolling of the ceramic ball. Otherwise, the rolling of the ceramic ball will be hindered, and the ceramic ball will slide in the V-shaped groove, which will easily cause scratches on the surface of the ceramic ball, and even cause excessive grinding of a certain part of the ceramic ball, affecting the roundness of the ceramic ball. In addition, if the number of the ceramic balls in the V-shaped groove is too large, some of the ceramic balls will jump out of the abrasive addition port. However, if the number of the ceramic balls in the V-shaped groove is too small, there will be no ceramic balls supporting part of the area between the fixed disk and the rotating disk, and the fixed disk will tilt, which is not conducive to processing. Therefore, during processing, there are certain requirements for the number of ceramic balls in the V-shaped groove. In a specific embodiment, when the diameters of the fixed disk and the rotating disk are 500 mm, the number of ceramic balls with a diameter of 28 mm in a single V-shaped groove is 45, and the number of ceramic balls with a diameter of 32 mm in a single V-shaped groove is 39; when the diameters of the fixed disk and the rotating disk are 800 mm, the number of ceramic balls with a diameter of 28 mm in a single V-shaped groove is 78, and the number of ceramic balls with a diameter of 32 mm in a single V-shaped groove is 68.
[0081] In some embodiments of the present invention, a V-groove is provided on a side of the rotating disk close to the fixed disk, and the ceramic ball is placed in the V-groove for processing. The ceramic ball rolls in the V-groove with the same linear speed, which is beneficial to batch size precision control of the ceramic balls; a plurality of V-grooves are provided on a side of the rotating disk close to the fixed disk, and the ceramic ball is placed in the V-grooves for processing. The number of ceramic balls in the V-grooves increases, but the spheres of the ceramic balls roll in different V-grooves with different linear speeds and different removal amounts. In order to ensure batch size control, the ceramic balls should be frequently turned over at the abrasive addition port to prevent the ceramic balls from always rolling in the same V-groove.
[0082] In some embodiments of the present invention, when the ceramic ball is ground in the V-groove, the V-groove also includes abrasives and grinding liquid, and the abrasives have the following properties: the shape and size of the abrasives are uniform; the abrasives can be properly crushed to make the cutting edge sharp; the abrasives are easily dispersed in the grinding liquid.
[0083] In some embodiments of the present invention, the abrasive includes corundum, boron carbide and diamond. The hardness of the abrasive is an important parameter for measuring the abrasive. In the grinding process of the ceramic ball, the hardness of the abrasive is higher than the hardness of the ceramic ball, and the higher the hardness of the abrasive, the more conducive it is to the removal of ceramic materials. The Brinell hardness of the diamond is 10000HB, the Brinell hardness of the boron carbide is 4000-5000HB, and the Brinell hardness of the corundum is 2000-2500HB.
[0084] In some embodiments of the present invention, another important indicator for measuring the performance of the abrasive is the particle size of the abrasive, that is, the size of the abrasive; when the particle size of the abrasive is large, the surface roughness of the ceramic ball is large, but the grinding efficiency is high. This is because as the particle size of the abrasive increases, the grinding depth of the ceramic ball increases accordingly, and the removal rate per unit time also increases accordingly, resulting in the surface of the ceramic ball being relatively rough. Therefore, the grinding process of the ceramic ball should gradually reduce the particle size of the abrasive to gradually improve the surface quality of the ceramic ball; the particle size of the abrasive should be selected based on the batch size and surplus of the ceramic ball blank, and gradually transitioned to ensure that the defects left over from the previous process are eliminated; the addition of the abrasive should follow the principles of "small amounts and multiple times" and "adding the grinding liquid first and then the abrasive".
[0085] In some embodiments of the present invention, the particle size of the abrasive is usually expressed by mesh number, and mesh refers to the number of holes on the screen per inch; 50 mesh means that there are 50 holes on the screen per inch, and the number of holes per square inch is 50*50=2500; the higher the mesh number, the more holes; when the particle size is expressed by mesh number, it refers to the particle size of the material that can pass through the screen, and the higher the mesh number, the smaller the particle size; there is a simple conversion formula between particle size and mesh number: particle size (μm) = 15000 ÷ mesh number. Specifically, the selection of the abrasive should consider both the mechanical strength of the ceramic ball and the price cost of the abrasive. At present, the abrasives used in the processing and production of the ceramic ball mainly include 60 mesh corundum, 600 mesh corundum, 3.5μm diamond grinding paste and 1μm diamond grinding paste and rare earth polishing agent, and all abrasives can be purchased on the market.
[0086] In some embodiments of the present invention, during the grinding process of the ceramic ball, the grinding fluid plays the role of lubrication, cooling, evenly distributing abrasives on the workpiece surface and removing chips. The grinding fluid has the following requirements: it should have a lower viscosity to improve the grinding efficiency; it should be able to mix well with the abrasives and facilitate the suspension of the abrasives to obtain a better grinding effect; it should have stable chemical and physical properties and will not decompose or deteriorate due to storage or temperature increase.
[0087] In some embodiments of the present invention, the grinding fluid includes water-based grinding fluid and oil-based grinding fluid. According to requirements and actual production conditions, the ceramic ball mainly adopts the water-based grinding fluid in the grinding process. The water-based grinding fluid is a mixture of an emulsifier, a rust inhibitor, a lubricant and an activator. The addition of the grinding fluid should also follow the principle of small amounts and multiple times rather than large amounts and few times. All grinding fluids can be purchased on the market, preferably from Hubei Yunsheng Rolling Body Manufacturing Co., Ltd.
[0088] In some embodiments of the present invention, there is a grinding pressure between the fixed disk and the rotating disk, and the grinding pressure has two functions in the grinding process of the ceramic ball: on the one hand, it makes the ceramic ball fully rotate; on the other hand, it grinds and squeezes the ceramic ball. Therefore, the grinding efficiency increases with the increase of the grinding pressure, but the spherical error of the ceramic ball also increases accordingly. Therefore, the selection of the grinding pressure should take both aspects into consideration. The grinding efficiency increases with the increase of the grinding pressure, but when the grinding pressure exceeds a certain range, it will have an adverse effect: the abrasive particles are hard and brittle materials, and when they cannot withstand the excessive grinding pressure, the abrasive particles will break and become finer; when the grinding pressure is too large, the friction between the ceramic ball and the fixed disk and the rotating disk increases, making the ceramic ball unable to rotate freely, especially slowing down the movement and change of the rotation axis of the ceramic ball and the rotation rate, thereby reducing the spherical accuracy and surface roughness of the ceramic ball. The grinding pressure range is 2-5MPa, which needs to be appropriately adjusted according to the removal rate in combination with the abrasive. The removal rate of the ceramic ball can be maintained at 10-5μm / hour in the rough grinding stage, about 0.3μm / hour in the fine grinding stage, and no more than 0.2μm / hour in the fine polishing stage. When the abrasive is just started to be changed, the removal rate should be faster. As the surface of the ceramic ball becomes smoother and smoother, the removal rate will gradually decrease. The fine polishing stage does not pursue a high removal rate, but needs to focus on the removal of surface defects of the ceramic ball, so that the surface morphology of the ceramic ball is improved.
[0089] In some embodiments of the present invention, the rotation speed of the rotating disk affects both the revolution and the rotation of the ceramic ball, thereby affecting the number of grinding times and grinding efficiency of the ceramic ball per unit time. When the rotation speed of the rotating disk is too large, the vibration of the rotating disk increases significantly, and the grinding efficiency and grinding quality decrease. This is because the rotation speed of the rotating disk increases, the vibration of the rotating disk increases, the spin of the ceramic ball is uneven, the efficiency is reduced, and the spherical error of the ceramic ball increases. From coarse to fine, taking into account the comprehensive influence of efficiency and processing accuracy, the rotation speed of the rotating disk should be gradually reduced. During the coarse grinding process, the rotation speed of the rotating disk is 30-50r / min; during the fine grinding process, the rotation speed of the rotating disk is 20-40r / min; during the fine treatment, the rotation speed of the rotating disk is 20-40r / min, and the fine treatment includes the first fine treatment and the second fine treatment.
[0090] In some embodiments of the present invention, the grinding process of the ceramic ball is divided into coarse grinding, fine grinding, fine processing and fine polishing, and the fine processing includes a first fine processing and a second fine processing; in the coarse grinding process, the abrasive used is coarse and the grinding pressure is large. It is an important process that affects the processing efficiency of the ceramic ball to complete about 95% of the processing volume of the ceramic ball. Therefore, it is necessary to increase the processing speed as much as possible while ensuring the processing quality of the ceramic ball; the fine grinding process is to refine the surface processing defects of the ceramic ball formed in the coarse grinding stage, improve the surface quality and precision of the ceramic ball, and lay the foundation for subsequent polishing. The particle size and grinding pressure of the abrasive used in the fine grinding process are both small, and the dimensional accuracy of the ceramic ball after fine grinding is high. , spherical accuracy and surface quality are generally close to the requirements of finished products; fine polishing is to improve the surface roughness and roundness of ceramic balls, and to remove the processing damage layer as much as possible, and reduce surface defects (such as surface scratches, pitting, etc.), which is very important to the quality of ceramic balls. Fine polishing generally uses abrasives below 1μm, and the rotation speed should not be too fast. Too fast a rotation speed can easily cause the ceramic balls to slide and create new scratches on the surface of the ceramic balls. The elastic-plastic deformation and tiny cracks in the processing metamorphic layer can be considered to be part of the mechanical energy used to generate chips. Therefore, from the perspective of the development of precision machining technology, it is very important to adopt chip generation conditions that make both the surface roughness and the processing metamorphic layer small.
[0091] In some embodiments of the present invention, the surface inspection process of the ceramic ball includes: after cleaning the ceramic ball, checking the surface condition of the ceramic ball particle by particle; as needed, further observing and analyzing the surface morphology of the ceramic ball by using an optical microscope and a scanning electron microscope; during the processing, the main surface defects of the ceramic ball include scratches, pitting, peeling pits, flat heads and cracks; for the ceramic balls with a diameter of 28 mm and a diameter of 32 mm, they are generally inspected under fluorescent lights, and visual inspection is required to be free of defects.
[0092] In some embodiments of the present invention, the diameter detection process of the ceramic ball includes: the diameter measuring instruments of the ceramic ball include a vernier caliper, a micrometer, a three-needle instrument and a special diameter measuring instrument. In actual production, different measuring instruments are selected according to needs.
[0093] In some embodiments of the present invention, the roundness detection process of the ceramic ball includes: roundness is the difference between the maximum radius and the minimum radius of the contour of the measured part, which indicates the degree to which the cross section of the workpiece is close to the theoretical circle. It is a method to characterize the spherical error of the ceramic ball. The smaller the roundness of the ceramic ball, the closer the ceramic ball is to an ideal sphere. According to the relevant standard GB / T308.2 for ceramic bearing balls, the least squares method is used to test the roundness to characterize the spherical error of the ceramic ball.
[0094] In some embodiments of the present invention, the surface roughness detection process of the ceramic ball includes: surface roughness refers to the unevenness of the machined surface with small spacing and tiny peaks and valleys, and the distance (wave pitch) between two wave peaks or two wave valleys is very small, which belongs to the microscopic geometric shape error. The smaller the surface roughness of the ceramic ball, the smoother the surface of the ceramic ball. Usually, the morphological features with a wave pitch less than 1 mm are attributed to surface roughness. According to the relevant standard GB / T 10610 for ceramic bearing balls, the surface roughness of the ceramic ball is tested.
[0095] In Example 1, Example 2, Example 3 and Example 4 of the present invention, the processing parameters of the ceramic femoral head during the processing are shown in Table 1.
[0096] Table 1 Processing parameters
[0097]
[0098] In some embodiments of the present invention, the parameters of the ceramic rough ball are shown in Table 2.
[0099] Table 2 Parameters of ceramic blank ball
[0100]
[0101]
[0102] The torque of the machining equipment in Example 1, Example 2, Example 3, Example 4 and Example 5 of the present invention is: 10Nm, the spindle processing speed of the machining equipment is 15000 rpm, the grinding wheel adopts a diamond grinding wheel, and the ceramic ball is fixed on the turntable of the machine tool and rotates with the turntable at a low speed (80r / min). While the grinding wheel rotates at a high speed, the tool descends along the generatrix of the tapered hole to complete the tapered hole processing.
[0103] Example 1
[0104] The material of the ceramic femoral head is zirconia reinforced alumina femoral head, the diameter of the fixed plate and the rotating plate is 500mm, the diameter of the powder ceramic blank ball is 28mm, the processing allowance is 30-50 threads, 220 balls / plate, 15-20 days for a production cycle, and the productivity is 11-14 balls / unit day (24 hours). The spindle torque of the mechanical processing equipment for processing the cone hole of the powder ceramic ball is 10Nm, and the cone hole of one ball is ground in 0.45 hours, and the productivity is 50 balls / unit day (24 hours); the angle α of the V-groove of the first processing equipment, the second processing equipment, the third processing equipment and the fourth processing equipment is 90°; the grinding fluid is a mixture of an emulsifier, a rust inhibitor, a lubricant and an active agent.
[0105] The combined efficiency is 11-14 pellets / day (24 hours), and the processing equipment and mechanical processing equipment are used in a 1:1 matching manner.
[0106] The specific processing process of ceramic femoral head is described as follows:
[0107] Rough grinding: according to Figure 2 According to the requirements, 220 powder ceramic balls with a diameter of 28 mm and a processing allowance of 30-50 silk are loaded into the V-groove of the first processing equipment. At the same time, the coarse abrasive and the grinding liquid are put into the V-groove of the first processing equipment. The speed of the first processing equipment is 40r / min. The grinding pressure of the powder ceramic balls is 3MPa. The temperature of the coarse grinding treatment is 40 degrees Celsius. The grinding liquid is a mixture of emulsifier, rust inhibitor, lubricant and activator. During the processing, the powder ceramic balls can be taken out and measured with a vernier ruler. The diameter is measured to determine the removal rate of the grinding process. When the diameter reaches 28 mm and the machining allowance is 30-100 μm, the rough grinding process is terminated to obtain a rough-ground powdered ceramic blank ball. The roundness of the rough-ground powdered ceramic blank ball is controlled within 0.1 mm. The removal rate of the rough grinding process is maintained at 5-10 μm / hour. The material of the first processing equipment is cast iron. The notch width of the V-shaped groove of the first processing equipment is greater than the diameter of the powdered ceramic blank ball. The rough grinding process lasts for 6 days. The coarse abrasive is 60-600 mesh corundum.
[0108] Fine grinding: replace the fixed disk and rotating disk on the first processing equipment, install new fixed disk and rotating disk to form the second processing equipment. The size and shape of the V-groove of the second processing equipment are the same as those of the first processing equipment. Then put the coarsely ground ceramic blank ball into the V-groove of the second processing equipment, and put the fine abrasive and grinding liquid into the V-groove of the second processing equipment. The speed of the second processing equipment is 30r / min, the grinding pressure of the coarsely ground ceramic blank ball is 2MPa, and the temperature of fine grinding is 35 degrees Celsius. During the processing, the coarse ground powder can be taken out. The diameter of the ceramic blank ball is measured with a vernier caliper to determine the removal rate of the grinding process. When the diameter reaches 28 mm and the machining allowance is 5-30 microns, the fine grinding process is completed to obtain a finely ground ceramic blank ball. The roundness of the finely ground ceramic blank ball is controlled at 5-10 microns, and the removal rate of the fine grinding process is maintained at 0.3 microns / hour. The material of the second processing equipment is cast iron, and the notch width of the V-groove of the second processing equipment is greater than the diameter of the coarsely ground ceramic blank ball. The fine grinding process lasts for 3 days, and the fine abrasive is a diamond grinding paste with a particle size of 0.35 microns or a boron carbide with a particle size of 3.5 microns.
[0109] Fine grinding treatment: replace the fixed disk and rotating disk on the second processing equipment, install new fixed disk and rotating disk to form the third processing equipment. The size and shape of the V-groove of the third processing equipment are the same as those of the second processing equipment. Then put the finely ground ceramic blank ball into the V-groove of the third processing equipment, and put the finely ground material and grinding liquid into the V-groove of the third processing equipment. The speed of the third processing equipment is 30r / min, the grinding pressure of the finely ground ceramic blank ball is 2MPa, and the temperature of the fine grinding treatment is 35 degrees Celsius. During the processing, the finely ground powder can be taken out. The diameter of the ceramic blank ball is measured by a three-needle instrument to determine the removal rate of the grinding process. When the diameter reaches 28 mm and the machining allowance is 1-5 microns, the fine grinding process is completed to obtain a finely ground ceramic blank ball. The roundness of the finely ground ceramic blank ball is controlled within 0.5 microns, and the removal rate of the fine grinding process is maintained at 0.3 microns / hour. The material of the third processing equipment is cast iron, and the notch width of the V-groove of the third processing equipment is greater than the diameter of the finely ground ceramic blank ball. The fine grinding process time is 10 hours, and the fine grinding material is a diamond grinding paste with a diameter of 1 micron or boron carbide of about 1 micron.
[0110] Fine polishing treatment, replace the fixed disk and the rotating disk on the third processing equipment, install new fixed disk and rotating disk to form a fourth processing equipment, the size and shape of the V-groove of the fourth processing equipment are the same as the V-groove of the third processing equipment, then put the fine-ground ceramic blank ball into the V-groove of the fourth processing equipment, and put the alumina polishing agent into the V-groove of the fourth processing equipment at the same time, the rotation speed of the fourth processing equipment is 30r / min, the grinding pressure of the fine-ground ceramic blank ball is 2MPa, the temperature of fine polishing treatment is 35 degrees Celsius, during the processing, the fine-ground ceramic blank ball can be taken out and the diameter is measured by a three-needle instrument to judge the removal rate of grinding, and the fine polishing treatment is terminated when the diameter is 28 mm and the diameter tolerance is -0.1-0.1 micron to obtain a ceramic ball, the roundness of the ceramic ball is controlled within 0.3 micron, and the removal rate of fine polishing treatment is maintained at 0.2 micron / hour, the material of the fourth processing equipment is cast iron, the notch width of the V-groove of the fourth processing equipment is greater than the diameter of the fine-ground ceramic blank ball, and the fine polishing treatment time is 10 hours;
[0111] Machining: Install a single ceramic ball in the fixture of the machining equipment and move it to the machining position. Install one ball in each fixture and only process one ball each time the tapered hole is ground. The time for grinding the tapered hole is 0.45 hours. The spindle speed of the machining equipment is 15,000 rpm and the spindle torque of the machining equipment is 10 Nm. After the machining is completed, a ceramic femoral head is obtained. The ceramic femoral head meets the requirements specified in the Medical Industry Standard of the People's Republic of China: YY0118-2016, Joint Replacement Implants and Membranous Joint Prostheses.
[0112] Example 2
[0113] The material of the ceramic femoral head is zirconia reinforced alumina femoral head. The diameter of the fixed plate and the rotating plate is 800mm, the diameter of the powder ceramic ball is 28mm, the processing allowance is 30-50 wires, 360 balls / plate, 15-20 days is a production cycle, and the productivity is 18-24 balls / unit day (24 hours); the spindle torque of the machining equipment is 10Nm, and it takes 0.45 hours to grind a tapered hole of a ceramic ball, with a productivity of 50 balls / unit day (24 hours).
[0114] The combined efficiency is 18-24 balls / day (24 hours), and the processing equipment and mechanical processing equipment are 1:1 matching.
[0115] The processing process is the same as that of Example 1.
[0116] Example 3
[0117] The material of the ceramic femoral head is zirconia reinforced alumina femoral head. The diameter of the fixed plate and the rotating plate is 1200mm, the diameter of the powder ceramic ball is 28mm, the processing allowance is 30-50 wires, 900 balls / plate, 15-20 days is a production cycle, and the productivity is 45-60 balls / unit day (24 hours); the spindle torque of the machining equipment is 10Nm, and it takes 0.45 hours to grind a tapered hole of a ceramic ball, with a productivity of 50 balls / unit day (24 hours).
[0118] The combined efficiency is 50 balls / unit day (24 hours), and the processing equipment and mechanical processing equipment are 1:1 matching.
[0119] The processing process is the same as that of Example 1.
[0120] Example 4
[0121] The material of the ceramic femoral head is zirconia reinforced alumina femoral head. The diameter of the fixed plate and the rotating plate is 1200mm, the diameter of the powder ceramic ball is 32mm, the processing allowance is 30-50 wires, 700 balls / plate, 15-20 days as a production cycle, and the productivity is 35-46 balls / unit day (24 hours); the spindle torque of the machining equipment is 10Nm, and it takes 0.45 hours to grind a ceramic ball's tapered hole, with a productivity of 50 balls / unit day (24 hours).
[0122] The combined efficiency is 35-46 pellets / day (24 hours), and the processing equipment and mechanical processing equipment are 1:1 matched.
[0123] The processing process is the same as that of Example 1, except that Figure 3 Grinding process is required.
[0124] Example 5
[0125] The material of the ceramic femoral head is silicon nitride, also known as silicon nitride ceramic femoral head, which is commonly known as "black pottery". The diameter of the fixed disk and the rotating disk is 1200mm, the diameter of the black pottery ball is 32mm, the processing allowance is 30-50 threads, 700 particles / disk, 25-28 days as a production cycle, and the productivity is 25-28 balls / unit day (24 hours); the spindle torque of the machining equipment is 30Nm, and it takes 2 hours to grind the tapered hole of a ceramic ball, with a productivity of 12 balls / unit day (24 hours).
[0126] The combined efficiency is 12 balls / day (24 hours), and the processing equipment and mechanical processing equipment are 1:1 matched.
[0127] The processing process is the same as that of Example 1, except that Figure 3 Grinding process is required.
[0128] The production efficiency of the above embodiments is closely related to the size and material of the processed ball and the size of the equipment used. The smaller the ball, the higher the production efficiency. The larger the diameter of the grinding disc used, the higher the production efficiency. The processing efficiency of pink pottery is higher than that of black pottery.
[0129] Comparative Example:
[0130] Provide a spherical blank with a tapered hole (the outer diameter of the ball head is 28 or 32 mm); use a CNC machine to process the outer spherical surface, install the blank according to the tapered hole (adhesive is required between the tapered hole and the installation tapered rod), use a bowl-shaped sintered grinding wheel to grind the spherical blank with a tapered hole until the roundness of the outer spherical surface reaches about 5 microns, replace the bowl-shaped grinding wheel with a bowl-shaped cast iron, install felt (other materials such as flannel can also be used) in the bowl-shaped mouth, apply diamond grinding paste, and roughly grind the outer spherical surface, and then perform fine grinding and fine polishing in turn until the roundness of the outer spherical surface reaches 0.5 microns and the surface roughness reaches Ra 0.05~0.1(um) micron; This process takes 2-3 hours to grind powder pottery and 3-4 hours to grind black pottery. Remove the spherical body with a tapered hole from the CNC machine tool, remove the installation cone rod from the tapered hole by dissolution or heating melting, and process the tapered hole again. The processing method is similar to that of Examples 1, 2, and 3. The main shaft torque is 10Nm. It takes 0.35 hours to grind the "powder pottery" tapered hole and 1.05 hours to grind the "black pottery" tapered hole. The production efficiency of this processing method has little to do with the size of the processed ball and the size of the equipment used. Compared with the embodiment of the present invention, its productivity: 8-12 balls / day for powder pottery and 6-8 balls / day for black pottery (24 hours), and the processing equipment and mechanical processing equipment are matched in a 1:1 ratio.
[0131] It can be seen from the comparative examples that the method of the patent improves the processing efficiency by more than 2 times, and the processing efficiency will increase with the increase of the diameter of the fixed disk and the rotating disk of the processing equipment.
[0132] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A processing technology for a ceramic femoral head, characterized in that: The following steps are involved: S0: providing a ceramic blank ball, wherein the material of the ceramic blank ball includes at least one of zirconium oxide reinforced aluminum oxide, silicon nitride, aluminum oxide, zirconium oxide and silicon carbide; S1: grinding the ceramic rough ball to obtain a ceramic ball; S2: Mechanically processing the ceramic ball to obtain the ceramic femoral head.
2. The processing technology according to claim 1, characterized in that: The abrasive for the grinding process is at least one of diamond, boron carbide, cubic boron nitride and silicon carbide, the grinding liquid for the grinding process is any one of water-based grinding liquid and oil-based grinding liquid, the grinding pressure for the grinding process is 2-5MPa, and the grinding temperature for the grinding process is 0-50°C.
3. The processing technology according to claim 1 or 2, characterized in that: The grinding process includes coarse grinding, fine grinding, lapping and polishing in sequence; The rough grinding process includes: placing the ceramic blank ball into a first processing device for rough grinding to obtain a rough ground ceramic blank ball; The fine grinding process comprises: placing the coarsely ground ceramic blank ball into a second processing device for fine grinding to obtain a finely ground ceramic blank ball; The lapping process comprises: placing the finely ground ceramic blank ball into a third processing device for lapping to obtain a lapping ceramic blank ball; The fine polishing treatment includes: placing the finely ground ceramic blank ball into a fourth processing device for fine polishing to obtain the ceramic ball.
4. The processing technology according to claim 3, characterized in that: The step of placing the ceramic blank ball into a first processing device for rough grinding to obtain a rough ground ceramic blank ball specifically comprises the following steps: placing the ceramic blank ball into the first processing equipment; placing a coarse abrasive in the first processing equipment; The rotation speed of the first processing equipment is set to 30-50 r / min to rough-grind the ceramic blank ball to obtain the rough-grinded ceramic blank ball.
5. The processing technology according to claim 3, characterized in that: The step of placing the coarsely ground ceramic blank ball into a second processing device for fine grinding to obtain a finely ground ceramic blank ball specifically comprises the following steps: placing the roughly ground ceramic blank ball into the second processing equipment; placing fine abrasive in the second processing equipment; The rotation speed of the second processing equipment is set to 20-40 r / min to finely grind the coarsely ground ceramic blank ball to obtain the finely ground ceramic blank ball.
6. The processing technology according to claim 3, characterized in that: The step of placing the finely ground ceramic blank ball into a third processing device for fine grinding to obtain a finely ground ceramic blank ball specifically comprises the following steps: placing the finely ground ceramic rough ball into the third processing equipment; placing finely ground material into the third processing equipment; The rotation speed of the third processing equipment is set to 20-40 r / min to grind the fine-ground ceramic blank ball to obtain the grinded ceramic blank ball.
7. The processing technology according to claim 3, characterized in that: The step of placing the finely ground ceramic rough ball into a fourth processing device for fine polishing to obtain the ceramic ball specifically comprises the following steps: placing the finely ground ceramic blank ball into the fourth processing equipment; placing a polishing agent in the fourth processing equipment; The rotation speed of the fourth processing equipment is set to 20-40 r / min to perform fine polishing on the finely ground ceramic blank ball to obtain the ceramic ball.
8. The processing technology according to claim 3, characterized in that: The first processing equipment is added with coarse abrasive, the mesh size of which is 60-600 meshes, the second processing equipment is added with fine abrasive, the particle size of which is 3-5 microns, and the third processing equipment is added with fine abrasive, the particle size of which is 0.8-1.2 microns.
9. The processing technology according to claim 8, characterized in that: The coarse abrasive includes diamond with a mesh size of 60-600 meshes, the fine abrasive includes diamond with a particle size of 3-5 microns, and the fine abrasive includes diamond with a particle size of 0.8-1.2 microns.
10. The processing technology according to claim 3, characterized in that: The removal rate of the ceramic blank ball in the rough grinding process is 5-10 microns / hour, the removal rate of the rough ground ceramic blank ball in the fine grinding process is 0.1-0.6 microns / hour, the removal rate of the fine ground ceramic blank ball in the fine grinding process is 0.1-0.6 microns / hour, and the removal rate of the fine ground ceramic blank ball in the fine polishing process is 0.1-0.3 microns / hour.
11. The processing technology according to claim 3, characterized in that: The machining allowance of the ceramic blank ball is 30-50 microns, the machining allowance of the coarsely ground ceramic blank ball is 30-100 microns, the machining allowance of the finely ground ceramic blank ball is 5-30 microns, the machining allowance of the finely ground ceramic blank ball is 1-5 microns, and the diameter tolerance of the ceramic ball after fine polishing is -0.1-0.1 microns.
12. The processing technology according to claim 1, characterized in that: The specific steps of mechanically processing the ceramic ball to obtain the ceramic femoral head include: grinding a plane on the ceramic ball, and sequentially performing hole grinding, grinding and chamfering on the plane to obtain the ceramic femoral head.
13. A ceramic femoral head processing device, characterized in that: The grinding process described in any one of claims 1 to 12 is carried out in the processing equipment, which includes a base, a fixed disk, a rotating disk, a rotating shaft and a driving device. The fixed disk is fixedly connected to the base, the rotating disk is fixedly connected to the rotating shaft, and the rotating shaft rotates under the drive of the driving device and drives the rotating disk to rotate. A plurality of V-shaped grooves are provided on a side of the rotating disk close to the fixed disk.
14. The processing equipment according to claim 13, characterized in that The angle of the V-shaped groove is 70°-90°, the horizontal distance between the center axis of the V-shaped groove and the center axis of the fixed disk is less than 10°, and the horizontal distance between the center axis of the V-shaped groove and the center axis of the rotating disk is less than 10°.
Citation Information
Patent Citations
Machining device of outside spherical surface
CN102059618A
Artificial hip joint ceramic ball head synchronous on-line detecting processing device and method
CN108296929A
Surface-enhanced ceramic artificial joint convex spherical friction part and preparation method thereof
CN114409383A
Grinding process for high-precision V-shaped groove of ceramic ball
CN117245455A
Spherical body grinding method
JP2000254858A