Preparation method of composite current collector
By evenly applying glue on the polymer film and heating and hot pressing to tightly combine the metal particles, the problem of metal layer peeling is solved, the adhesion of the composite current collector and the energy density of the lithium battery are improved, and efficient composite current collector preparation is achieved .
Patent Information
- Application Number
- CN202410820019.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing vacuum coating and water plating methods often cause problems such as metal layer peeling and poor adhesion when preparing composite current collectors, which affects the energy density and lightweight requirements of lithium batteries.
The surface of the polymer film is evenly coated with glue and covered with metal particles. After heating and hot pressing, it is tightly combined to ensure strong adhesion between the metal particles and the polymer film, and then vacuum coating or water plating is performed.
It achieves strong adhesion of the metal layer, reduces the resistivity of the composite current collector, increases the energy density of lithium batteries, simplifies equipment, reduces production costs and improves production efficiency.
Smart Images

Figure CN118721809A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of vacuum coating, and in particular to a method for preparing a composite current collector. Background Art
[0002] With the continuous development of the lithium-ion battery industry, people are increasingly pursuing high energy density and lightweight batteries. As an important component of the battery, reducing the mass of the current collector is an effective method. At present, the method of reducing the mass of the current collector is mainly to prepare a composite current collector by plating a conductive metal layer on the surface of the polymer film support layer; in the actual verification process, conventional vacuum coating methods and water electroplating will cause metal layer peeling and poor metal layer adhesion.
[0003] Therefore, it is necessary to invent a method for preparing a composite current collector. Summary of the invention
[0004] To this end, the present invention provides a method for preparing a composite current collector to solve the problems in the background technology.
[0005] In order to achieve the above object, the present invention provides the following technical solution: a method for preparing a composite current collector, comprising the following steps:
[0006] S1, passing the polymer film from the unwinding position through the roller system to the winding position, adjusting the angle of the flattening roller of the unwinding device, and ensuring that there are no wrinkles on the surface of the film layer;
[0007] S2, evenly apply a thin layer of glue on the surface of the polymer film, and then spread a layer of metal particles to ensure that the glue is completely covered by the metal particles; the polymer film covered with metal particles is passed through a slit to remove excess metal particles, ensuring the overall flatness of the film while also controlling the overall thickness of the film;
[0008] S3, the film material enters the oven and is heated. The heating temperature is controlled at 40-100°C to ensure that the polymer film does not soften while accelerating the curing of the glue. During the heating process of the oven, due to the action of the pressure roller, the metal particles are tightly combined with the polymer film layer. The film is then removed from the oven for cooling and shaping.
[0009] S4, repeating the above steps S1-S3, performing the same treatment on the reverse side of the polymer, and obtaining a roll of composite foil material with a seed layer having strong adhesion, and then performing vacuum coating or water electroplating on the composite foil material to obtain a composite current collector.
[0010] Preferably, the metal particles in S2 are high-purity atomized spherical aluminum powder with a particle size of 1 μm-100 μm or high-purity atomized spherical copper powder with a particle size of 1 μm-100 μm.
[0011] Preferably, the polymer film in S1 is made by mixing one or more materials selected from the group consisting of polyethylene terephthalate, polyethylene, polypropylene, polyamide, polyimide, polyvinyl chloride, and polystyrene.
[0012] Preferably, the thickness of the polymer film in S1 is 1 μm-10 μm.
[0013] Preferably, the thickness of the polymer film in S1 is 2 μm-8 μm.
[0014] Preferably, the glue in S2 is a mixture of one or more of acrylic adhesive, polymer adhesive, hot melt adhesive, inorganic adhesive, pressure-sensitive adhesive, water-based adhesive, and polymer adhesive.
[0015] Preferably, the hot pressing method in S3 is to set multiple sets of hot rollers in the oven along the conveying direction of the laminated material, and perform hot pressing by the multiple sets of hot rollers.
[0016] Preferably, the seed layer in S4 is divided into an upper metal seed layer and a lower metal seed layer, and the thickness of the upper metal seed layer and the lower metal seed layer are both 0.1 μm-3 μm.
[0017] Preferably, the vacuum coating method in S4 may be one or a combination of vacuum evaporation coating, vacuum magnetron sputtering coating, and vacuum electron beam coating.
[0018] The beneficial effects of the present invention are:
[0019] The present invention makes the metal particles and the polymer film closely fit together by bonding, oven heating and hot pressing with hot pressing rollers. In the process of oven heating, the polymer film layer is reduced in thickness after hot pressing, so that the thickness of the finished composite current collector is reduced, thereby reducing the resistivity of the composite current collector and improving the energy density of the lithium battery. The preparation process of the present invention has the characteristics of simple equipment, low investment cost, high production efficiency and strong adhesion of the metal layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0021] The structures, proportions, sizes, etc. illustrated in this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with the technology. They are not used to limit the conditions under which the present invention can be implemented, and therefore have no substantial technical significance. Any structural modification, change in proportion or adjustment of size shall still fall within the scope of the technical contents disclosed in the present invention without affecting the effects and purposes that can be achieved by the present invention.
[0022] Figure 1 A schematic diagram of the equipment process for preparing the metal seed layer provided by the present invention;
[0023] Figure 2 A schematic diagram of the structure of a composite current collector provided by the present invention;
[0024] In the figure: 101, polymer film layer; 201, glue bin; 301, metal powder bin; 1, unwinding device; 2, pressure roller; 3, hot pressing roller; 4, oven; 5, hot pressing roller; 6, winding device; 7, polymer film; 8, glue layer; 9, seed layer; 10, metal coating. DETAILED DESCRIPTION
[0025] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0026] See attached Figure 1 -Attached Figure 2 The present invention provides a method for preparing a composite current collector, comprising the following steps:
[0027] S1, the polymer film 7 is fixed at the winding position through the roller system from the unwinding position, and the angle of the flattening roller of the unwinding device 1 is adjusted so that there are no wrinkles on the surface of the film layer;
[0028] S2, a thin layer of glue is evenly applied on the surface of the polymer film, and then a layer of metal particles is evenly applied to ensure that the glue is completely covered by the metal particles; the polymer film 7 covered with metal particles is passed through a slit to remove excess metal particles, thereby ensuring the overall flatness of the film and controlling the overall thickness of the film;
[0029] S3, the film material enters the oven 4 and is heated, and the heating temperature is controlled at 40-100°C to ensure that the polymer film does not soften while accelerating the curing of the glue. During the heating process of the oven 4, due to the action of the pressure roller 2, the metal particles are tightly combined with the polymer film layer 101, and then the film is removed from the oven 4 for cooling and shaping;
[0030] S4, repeating the above steps S1-S3, performing the same treatment on the reverse side of the polymer, and obtaining a roll of composite foil material with a seed layer 9 having strong adhesion, and then performing vacuum coating or water electroplating on the composite foil material to obtain a composite current collector;
[0031] Embodiment 1:
[0032] A 6 μm polyethylene terephthalate film and a 30 nm high-purity atomized spherical aluminum powder with a purity of 99.3% were bonded together using the above equipment, the pressure of the hot pressing roller was 200 N, the oven temperature was set to 80° C., and the holding time was 1.5 min; after double-sided hot pressing, the thickness of the composite film layer was 6.1 μm, and vacuum evaporation coating was then performed to obtain a double-sided composite aluminum foil with a total film thickness of 8.5 μm;
[0033] Example 2
[0034] A 4.5 μm polypropylene film and a 30 nm high-purity atomized spherical copper powder with a purity of 99.5% were bonded together using the above equipment, the pressure of the hot pressing roller was 180 N, the oven temperature was set to 70° C., and the holding time was 1 min; after double-sided hot pressing, the thickness of the composite film layer was 1.6 μm, and magnetron sputtering coating was then performed to obtain a double-sided composite copper foil with a total film thickness of 6.7 μm;
[0035] Example 3
[0036] A 4.5 μm polypropylene film and a 40 nm high-purity atomized spherical copper powder with a purity of 99.5% were bonded together using the above equipment, the pressure of the hot pressing roller was 180 N, the oven temperature was set to 75° C., and the insulation time was 1 min; after double-sided hot pressing, the thickness of the composite film layer was 1.7 μm, and then water electroplating was performed to obtain a double-sided composite copper foil with a total film thickness of 6.9 μm;
[0037] Comparative Example 1
[0038] The traditional positive electrode composite current collector commonly seen on the market is made by vacuum evaporation.
[0039] Comparative Example 2
[0040] The traditional negative electrode composite current collector commonly seen on the market is made by vacuum coating and electroplating.
[0041] The composite current collectors prepared in Examples 1-3 and Comparative Examples 1-2 were subjected to performance tests. The bonding strength test standard was as follows: the test sample was placed in an electrolyte and immersed for 48 hours, and then taken out and the bonding strength was tested using a tensile test machine. The electrolyte model was C15, the sample size was 15*100mm, and the test speed was 300mm / min. The test results are shown in the following table:
[0042]
[0043] By comparing the test results of Example 1 and Comparative Example 1 in the table, it can be seen that the positive electrode composite current collector prepared by the present invention has lower square resistance and resistivity, and the thickness of the positive electrode composite current collector is thinner; by comparing the test results of Examples 2 and 3 and Comparative Example 2 in the table, it can be seen that the negative electrode composite current collector prepared by the present invention has lower square resistance and resistivity, and the thickness of the negative electrode composite current collector is thinner, and the bonding strength passes the test.
[0044] The above is only a preferred embodiment of the present invention. Any person skilled in the art may modify the present invention by using the above technical solution or modify it into an equivalent technical solution. Therefore, any simple modification or equivalent replacement made according to the technical solution of the present invention belongs to the scope of protection claimed by the present invention.
Claims
1. A method for preparing a composite current collector, characterized in that: The following steps are involved: S1, passing the polymer film (7) from the unwinding position through a roller system and fixing it at the winding position, adjusting the angle of the flattening roller of the unwinding device (1) so that there are no wrinkles on the surface of the film layer; S2, a thin layer of glue is evenly applied on the surface of the polymer film, and then a layer of metal particles is evenly applied to ensure that the glue is completely covered by the metal particles; the polymer film (7) covered with metal particles is passed through a slit to remove excess metal particles, thereby ensuring the overall flatness of the film and controlling the overall thickness of the film material; S3, the film material enters the oven (4) and is heated, and the heating temperature is controlled at 40-100° C. to ensure that the polymer film does not soften while accelerating the curing of the glue. During the heating process of the oven (4), due to the action of the pressure roller (2), the metal particles and the polymer film layer (101) are tightly combined, and then the film is removed from the oven (4) to be cooled and shaped; S4, repeating the above steps S1-S3, and performing the same treatment on the reverse side of the polymer, so as to obtain a roll of composite foil material with a seed layer (9) having strong adhesion, and then performing vacuum coating or water electroplating on the composite foil material to obtain a composite current collector.
2. The method for preparing a composite current collector according to claim 1, characterized in that: The metal particles in S2 are high-purity atomized spherical aluminum powder with a particle size of 1 μm-100 μm or high-purity atomized spherical copper powder with a particle size of 1 μm-100 μm.
3. The method for preparing a composite current collector according to claim 1, characterized in that: The polymer film in S1 is made by mixing one or more materials selected from the group consisting of polyethylene terephthalate, polyethylene, polypropylene, polyamide, polyimide, polyvinyl chloride, and polystyrene.
4. The method for preparing a composite current collector according to claim 3, characterized in that: The thickness of the polymer film in S1 is 1 μm-10 μm.
5. The method for preparing a composite current collector according to claim 3, characterized in that: The thickness of the polymer film in S1 is 2 μm-8 μm.
6. The method for preparing a composite current collector according to claim 1, characterized in that: The glue in S2 is one or more of acrylic adhesive, polymer adhesive, hot melt adhesive, inorganic adhesive, pressure sensitive adhesive, water-based adhesive, and polymer adhesive.
7. The method for preparing a composite current collector according to claim 1, characterized in that: The hot pressing method in S3 is to set multiple sets of hot rollers in the oven (4) along the conveying direction of the laminated material, and perform hot pressing by the multiple sets of hot rollers.
8. The method for preparing a composite current collector according to claim 1, characterized in that: The seed layer (9) in S4 is divided into an upper metal seed layer and a lower metal seed layer, and the thickness of the upper metal seed layer and the lower metal seed layer are both 0.1 μm-3 μm.
9. The method for preparing a composite current collector according to claim 1, characterized in that: The vacuum coating method in S4 may be one or a combination of vacuum evaporation coating, vacuum magnetron sputtering coating, and vacuum electron beam coating.