Magnetic wave-absorbing honeycomb and preparation method thereof

By mixing hot-melt resin and magnetic absorber to make an absorbing film, and preparing a magnetic absorbing honeycomb through impregnation and lamination processes, the problems of complex molding process and environmental pollution in the existing technology are solved, and the absorption efficiency is improved. Wave effect and material uniformity.

CN118721894AActive Publication Date: 2024-10-01LUOYANG INST OF CUTTING EDGE TECH +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310350021.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

The existing magnetic wave-absorbing honeycomb molding process is complex, the molding process causes environmental pollution, and the wave-absorbing effect is poor.

Method used

The microwave-absorbing film is made by mixing hot-melt resin and magnetic absorbing agent. The magnetic absorbing honeycomb is prepared by impregnating aramid paper or fiber felt and combining viscose, lamination, stretching and curing processes to avoid the impregnation process. , simplifying the molding process.

Benefits of technology

The overall uniformity and wave absorption strength of the honeycomb are improved, the molding process is simplified, and environmental pollution is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721894A_ABST
    Figure CN118721894A_ABST
Patent Text Reader

Abstract

The invention provides a magnetic wave-absorbing honeycomb and a preparation method thereof. The preparation method comprises the following steps: S1, heating hot-melt resin to a molten state to obtain molten resin; s2, mixing the molten resin with a magnetic wave-absorbing agent to obtain a magnetic rubber material, and preparing the magnetic rubber material into a wave-absorbing rubber film; s3, carrying out impregnation treatment on the wave-absorbing adhesive film and aramid paper or a fiber felt to obtain a wave-absorbing impregnated felt; and S4, sequentially gluing, laminating, stretching and curing the wave-absorbing impregnated felt to obtain the magnetic wave-absorbing honeycomb. Hot-melt resin and a magnetic wave-absorbing agent are mixed to obtain a wave-absorbing adhesive film, the wave-absorbing adhesive film is impregnated with aramid paper or fiber felt to prepare a wave-absorbing impregnated felt, and then the magnetic wave-absorbing honeycomb is obtained through the processes of gluing, laminating, stretching, curing and the like. The impregnation technology is not involved in the honeycomb forming process, the forming technology is simple and environmentally friendly, and meanwhile the overall uniformity and the wave absorbing strength of the honeycomb are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of wave-absorbing materials, and in particular to a magnetic wave-absorbing honeycomb and a preparation method thereof. Background Art

[0002] With the rapid development of electronics and informatization, electromagnetic waves, as an important carrier of information transmission, have penetrated into all aspects of life. At the same time, the widespread application of electronic and electrical products in the information age has formed a complex electromagnetic environment and brought a lot of negative effects, such as misoperation caused by electromagnetic interference, information leakage, electromagnetic radiation, etc. In order to solve the above problems, absorbing materials with wide frequency band and high absorption have attracted more and more attention from scholars. At present, many different methods have been used to improve the absorption performance of absorbing materials, such as optimizing the content of absorbers, doping of different absorbers, and using multi-layer structure design. Existing experimental results show that the material can have the characteristics of "wide frequency band and high absorption" through structural design. Honeycomb structure has the advantages of light weight and high strength, and is widely used as a matrix design honeycomb absorbing material. Traditional absorbing honeycombs are mostly prepared by using aramid paper honeycombs as the matrix and impregnating absorbing slurry. Due to its special porous structure, the absorbing honeycomb prepared by this preparation method has a relatively complicated structural design process in the honeycomb hole, which is not conducive to large-scale production. Summary of the invention

[0003] The main purpose of the present invention is to provide a magnetic wave-absorbing honeycomb and a preparation method thereof, so as to solve the problems in the prior art of complex forming process of the magnetic wave-absorbing honeycomb, large environmental pollution during the forming process and poor wave-absorbing effect.

[0004] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing a magnetic absorbing honeycomb is provided, and the method comprises: step S1, heating a hot-melt resin to a molten state to obtain a molten resin; step S2, mixing the molten resin with a magnetic absorbing agent to obtain a magnetic adhesive, and making the magnetic adhesive into an absorbing adhesive film; step S3, subjecting the absorbing adhesive film to an impregnation treatment with aramid paper or fiber felt to obtain an absorbing impregnated felt; step S4, subjecting the absorbing impregnated felt to sequentially adhesive bonding, laminating, stretching and curing the absorbing impregnated felt to obtain a magnetic absorbing honeycomb.

[0005] Furthermore, in step S2, the weight ratio of the molten resin to the magnetic absorber is 20:1 to 1:2; preferably, the weight ratio of the molten resin to the magnetic absorber is 19:1 to 1:1.

[0006] Further, step S2 comprises: respectively mixing N kinds of molten resins with magnetic absorbers in different proportions to obtain N kinds of magnetic sizing materials, and making the N kinds of magnetic sizing materials into N kinds of absorbing adhesive films. Accordingly, when laminating in step S4, the N kinds of absorbing impregnated felts corresponding to the N kinds of absorbing adhesive films are arranged in order from low to high according to the content of the magnetic absorber therein, N=2 to 20; preferably, N=10 to 15; preferably, after the N kinds of magnetic sizing materials are arranged in order from small to large according to the content of the magnetic absorber, the content of the magnetic absorber in the two adjacent magnetic sizing materials differs by 3 to 5wt%.

[0007] Furthermore, the hot-melt resin is any one or more of hot-melt epoxy resin and bismaleimide resin; preferably, the viscosity of the hot-melt resin at 70° C. is 7000-16000 mPa·s, more preferably 14000-16000 mPa·s.

[0008] Furthermore, the magnetic wave absorbing agent includes any one or more of carbonyl iron powder, sendust aluminum alloy powder and ferrite.

[0009] Preferably, the average particle size of the Sendust aluminum alloy powder is 10-13 μm.

[0010] Preferably, the average particle size of the carbonyl iron powder is 5-10 μm.

[0011] Preferably, the average particle size of the ferrite is 1 to 5 μm.

[0012] Furthermore, the thickness of the wave-absorbing film is 0.1-0.2 mm.

[0013] Further, step S3 comprises: impregnating the absorbing adhesive film with aramid paper or fiber felt to obtain an absorbing prepreg felt, and keeping the absorbing prepreg felt at 80-90° C. for 60-70 minutes to obtain an absorbing feed felt; preferably, the impregnation is single-sided impregnation.

[0014] Furthermore, the fiber felt is aramid fiber felt.

[0015] Furthermore, the curing temperature is 80-160° C., and preferably, the curing includes: keeping warm at 80-85° C. for 55-60 min, keeping warm at 125-130° C. for 120-125 min, and keeping warm at 155-160° C. for 60-65 min.

[0016] According to another aspect of the present application, a magnetic wave-absorbing honeycomb is provided, and the magnetic wave-absorbing honeycomb is prepared by any one of the above-mentioned preparation methods.

[0017] By applying the technical solution of the present invention, a wave-absorbing adhesive film is obtained by mixing a hot-melt resin with a magnetic wave-absorbing agent, and a wave-absorbing impregnated felt is made by absorbing the impregnated adhesive film onto aramid paper or fiber felt, and then a magnetic wave-absorbing honeycomb is obtained through processes such as gluing, laminating, stretching and curing. The present application does not involve the impregnation process in the honeycomb forming process, and the forming process is simple and environmentally friendly, while the overall uniformity and wave-absorbing strength of the honeycomb are improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0019] Figure 1 A schematic diagram of the process flow of preparing a magnetic wave-absorbing honeycomb according to Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0020] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0021] As analyzed in the background technology of this application, there are problems in the prior art such as complex magnetic absorbing honeycomb molding process, large environmental pollution during the molding process and poor absorbing effect. In order to solve this problem, this application provides a magnetic absorbing honeycomb and a preparation method thereof.

[0022] According to a typical embodiment of the present application, a method for preparing a magnetic absorbing honeycomb is provided, and the method comprises: step S1, heating a hot-melt resin to a molten state to obtain a molten resin; step S2, mixing the molten resin with a magnetic absorbing agent to obtain a magnetic adhesive, and making the magnetic adhesive into an absorbing adhesive film; step S3, subjecting the absorbing adhesive film to an impregnation treatment with aramid paper or fiber felt to obtain an absorbing impregnated felt; step S4, subjecting the absorbing impregnated felt to sequentially gluing, laminating, stretching and curing the absorbing impregnated felt to obtain a magnetic absorbing honeycomb.

[0023] The present application obtains an absorbing adhesive film by mixing a hot-melt resin with a magnetic absorbing agent, and makes an absorbing impregnated felt by impregnating an aramid fiber paper or a fiber felt with the absorbing adhesive film, and then obtains a magnetic absorbing honeycomb by processes such as gluing, laminating, stretching, and curing. The present application does not involve an impregnation process in the honeycomb forming process, and the forming process is simple and environmentally friendly, while the overall uniformity and absorbing strength of the honeycomb are improved.

[0024] The ratio of the hot melt resin and the magnetic absorber in the absorbing film of the present application can be determined according to the specific use requirements, without any special restrictions. In some embodiments of the present application, in the above step S2, the weight ratio of the molten resin to the magnetic absorber is 20:1 to 1:2; especially when the weight ratio of the molten resin to the magnetic absorber is 19:1 to 1:1, the uniformity and absorbing effect of the prepared honeycomb material are better.

[0025] In some typical embodiments of the present application, in order to further improve the shortcomings of the absorbing honeycomb such as narrow absorption band and low absorption intensity, the above step S2 includes: respectively mixing N kinds of molten resins with magnetic absorbers in different proportions to obtain N kinds of magnetic adhesives, and making the N kinds of magnetic adhesives into N kinds of absorbing adhesive films; respectively impregnating the N kinds of adhesive films in aramid paper or fiber felt to obtain corresponding N kinds of absorbing impregnated felts, and when laminating in the next step S4, the N kinds of absorbing impregnated felts corresponding to the N kinds of absorbing adhesive films are arranged in order according to the content of magnetic absorbers therein, N=2~20. The absorption bandwidth and absorption intensity of the honeycomb can be effectively improved by introducing an impedance gradient structure. Preferably, N=10~15, and the above-mentioned performance of the prepared absorbing honeycomb is better.

[0026] In some preferred embodiments, after N kinds of magnetic adhesives are arranged in ascending order according to the content of magnetic absorber, the content of magnetic absorber in two adjacent magnetic adhesives differs by 3-5wt%; more preferably, after N kinds of magnetic adhesives are arranged in ascending order according to the content of magnetic absorber, the content of magnetic absorber in each adjacent two magnetic adhesives changes in the same way, that is, when N kinds of absorbing impregnated felts are laminated, the content of magnetic absorber in each layer of absorbing impregnated felt increases by a certain value between 3-5wt%, that is, the increasing gradient is a certain value between 3-5wt%. For example, the increasing gradient can be 3wt%, 3.5wt%, 3.8wt%, 4wt%, 4.2wt%, 4.5wt%, 4.8wt%, 5wt% or any range therebetween.

[0027] The hot-melt resin can be selected from the prior art, and it can be easily heated and melted to mix with the magnetic absorber. There is no special requirement. In some embodiments of the present application, the hot-melt resin is any one or more of hot-melt epoxy resin and bismaleimide resin. In particular, when hot-melt epoxy resin is used, it has good wrapping properties for the magnetic absorber, long operating time, and is more convenient for the implementation of the process. In some preferred embodiments, the viscosity of the hot-melt resin at 70°C is 7000-16000 mPa·s, which is more convenient for kneading with the magnetic absorber, and the impregnation effect is better, and the overall uniformity of the obtained magnetic honeycomb is better. More preferably, the viscosity of the hot-melt resin at 70°C is 14000-16000 mPa·s, especially when a hot-melt epoxy resin is used. When the viscosity is such, the overall performance of the magnetic honeycomb is particularly improved. Exemplarily, the viscosity of the hot-melt resin at 70°C is 8000 mPa·s, 9000 mPa·s, 10000 mPa·s, 11000 mPa·s, 12000 mPa·s, 13000 mPa·s, 14000 mPa·s, 14500 mPa·s, 15000 mPa·s, 15500 mPa·s, 16000 mPa·s or any range therebetween.

[0028] In the above step S1, a person skilled in the art can easily heat the hot-melt resin to a melted state according to the specific type and performance parameters of the selected hot-melt resin to obtain a molten resin, and then uniformly mix it with the magnetic absorber to prepare an absorbing adhesive film. In some embodiments of the present application, the viscosity of the hot-melt resin used at 70°C is 14000-16000 mPa·s. When performing step S1, the resin can be kept at 70-80°C for 30-35 minutes, for example, kept in an oven at 80°C for 30 minutes.

[0029] The magnetic wave absorbing agent can be selected from the prior art. In some embodiments of the present application, the magnetic wave absorbing agent includes any one or more of carbonyl iron powder, sendust aluminum alloy powder and ferrite, which is convenient for dispersion in the hot-melt resin, and the prepared wave absorbing honeycomb has better wave absorbing effect. Preferably, the average particle size of the sendust aluminum alloy powder is 10-13 μm, the average particle size of the carbonyl iron powder is 5-10 μm, and the average particle size of the ferrite is 1-5 μm, which is conducive to further improving the overall uniformity of the honeycomb.

[0030] In the above step S2, there are no special requirements for the method of mixing the magnetic absorbent and the above molten resin to obtain the magnetic adhesive and the method of preparing the magnetic adhesive into an absorbing adhesive film. The mixing method and the adhesive film preparation method of the prior art can be referred to. For example, the molten resin is introduced into a kneader, the kneader is turned on, the magnetic absorbent is added to mix evenly, and the mixed adhesive is poured into a film machine to prepare the absorbing adhesive film. In some embodiments of the present application, the thickness of the absorbing adhesive film is 0.1 to 0.2 mm, which is convenient for the preparation of the adhesive film and the implementation of subsequent processes.

[0031] In the above step S3, the above-mentioned absorbing adhesive film is combined with the aramid paper or fiber felt by impregnation. During the treatment process, the absorbing adhesive film can penetrate the surface and penetrate into the interior of the aramid paper or fiber felt. Combined with the subsequent bonding, curing and other complete treatment processes, a wide-band, high-absorption honeycomb material can be obtained without involving the impregnation treatment. The specific implementation method of the impregnation can refer to the prior art. In some embodiments of the present application, the heating temperature during the impregnation is 80-82°C and the pressure is 3-4MPa, so that the absorbing impregnated felt can be obtained efficiently.

[0032] In some preferred embodiments of the present application, the above step S3 includes: impregnating aramid paper or fiber felt with the absorbing adhesive film to obtain an absorbing prepreg felt, keeping the absorbing prepreg felt at 80-90°C for 60-70 minutes until it does not adhere to each other at room temperature, thereby obtaining an absorbing prepreg felt; heating and heat-insulating the impregnated absorbing prepreg felt, the absorbing feed felt can be initially cured, which is beneficial to further improve the overall uniformity and absorbing performance of the magnetic honeycomb, and is also convenient for subsequent processing. According to actual application requirements, double-sided impregnation or single-sided impregnation can be performed. In some embodiments of the present application, in order to improve the preparation efficiency, the above-mentioned impregnation is single-sided impregnation, that is, when performing the impregnation process, an absorbing adhesive film is set on one surface of the aramid paper or fiber felt for impregnation.

[0033] The aramid paper and fiber felt used for impregnation can be selected from the prior art. In some embodiments of the present application, the fiber felt is aramid fiber felt, also known as aramid fiber needle felt, which has better magnetic wave absorbing honeycomb performance. Preferably, the thickness of the aramid fiber felt is 0.1-0.2 mm.

[0034] After the above-mentioned absorbing feed felt is subjected to processes such as gluing, laminating, stretching and curing, a magnetic absorbing honeycomb with excellent absorbing performance can be obtained. The specific process methods of gluing, laminating, stretching and curing can refer to the existing technology and there are no special requirements. The technical personnel in this field can easily implement them, and they will not be introduced one by one here. In some embodiments of the present application, the curing temperature is 80-160°C, and the magnetic honeycomb material formed has good absorbing performance and high strength; the curing can also be carried out by programmed heating. Preferably, the temperature is kept at 80-85°C for 55-60 minutes, at 125-130°C for 120-125 minutes, and at 160-165°C for 60-65 minutes, which helps to further improve the comprehensive performance of the absorbing honeycomb.

[0035] According to another typical embodiment of the present application, a magnetic wave-absorbing honeycomb is provided, which is prepared by any of the above-mentioned preparation methods. The magnetic wave-absorbing honeycomb does not involve a dipping process during the honeycomb forming process, and the forming process is simple and environmentally friendly, while the overall uniformity and wave-absorbing strength of the honeycomb are improved.

[0036] The beneficial effects that can be achieved by the present application will be further illustrated below in combination with embodiments and comparative examples.

[0037] Example 1

[0038] The process flow of preparing the magnetic wave absorbing honeycomb in this embodiment is as follows: Figure 1As shown. Step 1: Put 300 grams of epoxy resin (brand name YPH160, viscosity of 14000mP.s at 70℃) into an oven at 80℃ for 30 minutes to melt. Step 2: Pour the melted resin into a kneader, open the kneader, add 5% of the weight of the epoxy resin carbonyl iron powder (15g, purchased from Jiangsu Tianyi Superfine Metal Powder Co., Ltd., average particle size 5μm), mix evenly, and obtain an absorbing adhesive. Step 3: Pour the evenly mixed absorbing adhesive into a film making machine to form a 0.1-0.12mm absorbing adhesive film for standby use, numbered P05. Repeat steps 2 and 3, increase the absorber content in a gradient of 5% of the weight of the epoxy resin, and prepare absorbing adhesive films with different magnetic absorber contents, numbered P05, P10, P15, P20, P25, P30, P35, P40, P45 and P50. Step 4: Place the prepared adhesive film and aramid fiber felt (purchased from Wuxi Wenqi Industry and Trade Co., Ltd.) in an impregnation machine for single-sided impregnation, set the impregnation machine heating temperature to 80°C and the pressure to 3MPa, and prepare P05-P50 absorbing prepreg felts, where the number of the absorbing prepreg felt is the same as the number of the absorbing adhesive film impregnated therein, and the same number is also used after the corresponding subsequent processing. Step 5: Put the prepared P05-P50 absorbing prepreg felts into an oven at 80°C for 60 minutes, until the absorbing prepreg felts are not adhered to each other at room temperature. Step six: Paste the P05-P50 absorbing impregnated felt with core strip glue at an interval of 1.8mm, and then stack them in order from large to small according to the absorbing impregnated felt number, place them at room temperature for 24 hours to solidify the glue strips, and then obtain a magnetic absorbing honeycomb intermediate with a honeycomb structure by stretching, and then keep the intermediate at 80℃ for 60min, 130℃ for 120min, and 160℃ for 60min, and solidify to obtain a magnetic absorbing honeycomb with a thickness of about 30mm and an impedance gradient structure.

[0039] Example 2

[0040] The only difference from Example 1 is that the carbonyl iron powder is replaced by sendust aluminum with an average particle size of 10 μm (Qinghe County Fengye Metal Materials Co., Ltd.).

[0041] Example 3

[0042] The only difference from Example 1 is that the carbonyl iron powder is replaced by ferrite with an average particle size of 5 μm (Qinghe County Benyu Metal Materials Co., Ltd.).

[0043] Example 4

[0044] The only difference from Example 1 is that the carbonyl iron powder is replaced by ferrite with an average particle size of 5 μm (Qinghe County Benyu Metal Materials Co., Ltd.) and sendustine with an average particle size of 10 μm (Qinghe County Fengye Metal Materials Co., Ltd.), wherein the weight ratio of sendustine to ferrite is 2:1.

[0045] Example 5

[0046] Step 1: Put 300 grams of epoxy resin (the same as in Example 1) into an oven at 80°C for 30 minutes to become a melted state. Step 2: Pour the melted resin into a kneader, open the kneader, add 50% of the weight of the epoxy resin carbonyl iron powder (150g, purchased from Jiangsu Tianyi Superfine Metal Powder Co., Ltd., with an average particle size of 5μm), and mix evenly. Step 3: Pour the evenly mixed absorbing adhesive into a film machine to form a 0.1-0.12mm absorbing adhesive film for standby use. Step 4: Place the prepared adhesive film and aramid fiber felt (the same as in Example 1) in an impregnation machine for single-sided impregnation, set the impregnation machine heating temperature to 80°C and the pressure to 3MPa, and prepare an absorbing prepreg felt. Step 5: Put the prepared absorbing prepreg felt into an oven at 80°C for 60 minutes until the absorbing prepreg felts are not adhered to each other at room temperature. Step six: Paste the absorbing impregnated felt with core strip glue with an interval of 1.8mm, then laminate the absorbing impregnated felt, place it at room temperature for 24 hours to solidify the glue strip, and then obtain a magnetic absorbing honeycomb intermediate with a honeycomb structure by stretching, and then keep it at 80℃ for 60min, 130℃ for 120min, and 160℃ for 60min to obtain a magnetic absorbing honeycomb with a thickness of about 30mm.

[0047] Example 6

[0048] The only difference from Example 1 is that the epoxy resin is YPH200T (viscosity at 70° C. is 15000 mP.s).

[0049] Example 7

[0050] The only difference from Example 1 is that the epoxy resin is replaced by liquid bismaleimide resin (purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., with a viscosity of 8000 mP.s at 25°C).

[0051] Example 8

[0052] The only difference from Example 1 is that the average particle size of the carbonyl iron powder is 10 μm.

[0053] Example 9

[0054] The only difference from Example 1 is that the aramid fiber felt in Example 1 is replaced by the para-aramid fiber felt produced by Shandong Xuzheng Textile Co., Ltd.

[0055] Example 10

[0056] The only difference from Example 1 is that the aramid fiber felt in Example 1 is replaced by aramid paper (YT822A meta-aramid paper).

[0057] Embodiment 11

[0058] The only difference from Example 1 is that: Steps 2 and 3 are repeated, and the content of the absorber is increased in a gradient of 7% of the weight of the epoxy resin.

[0059] Example 12

[0060] The only difference from Example 1 is that: Steps 2 and 3 are repeated, and the content of the absorber is increased in a gradient of 3% of the weight of the epoxy resin.

[0061] Embodiment 13

[0062] Step 1: Put 300 grams of epoxy resin (same as Example 1) into an oven at 80°C for 30 minutes to melt. Step 2: Pour the melted resin into a kneader, open the kneader, add 5% of the weight of the epoxy resin carbonyl iron powder (15g, purchased from Jiangsu Tianyi Superfine Metal Powder Co., Ltd.), mix well, and obtain an absorbing adhesive. Step 3: Pour the evenly mixed absorbing adhesive into a film making machine to make a 0.1-0.12mm absorbing adhesive film for standby use, numbered P05. Repeat steps 2 and 3, increase the absorber content in a gradient of 2% of the weight of the epoxy resin, and prepare absorbing adhesive films with different magnetic absorber contents, numbered P1, P2, P3...P20. Step 4: Place the prepared adhesive film and aramid fiber felt (purchased from Wuxi Wenqi Industry and Trade Co., Ltd.) in an impregnation machine for single-sided impregnation, set the impregnation machine heating temperature to 80°C and the pressure to 3MPa, and prepare absorbing prepreg felts numbered P1-P20, where the number of the absorbing prepreg felt is the same as the number of the absorbing adhesive film impregnated therein, and the same number is also used after the corresponding subsequent processing. Step 5: Place the prepared absorbing prepreg felts numbered P1-P20 in an oven at 80°C for 60 minutes until the absorbing prepreg felts are not adhered to each other at room temperature. Step six: glue the core strips of P1-P20 absorbing impregnated felts, and then stack them in order from large to small according to the absorbing impregnated felt numbers. Place them at room temperature for 24 hours to solidify the glue strips, and then stretch them to obtain a magnetic absorbing honeycomb intermediate with a honeycomb structure. Then, keep the intermediate at 80°C for 60 minutes, 130°C for 120 minutes, and 160°C for 60 minutes, and solidify it to obtain a magnetic absorbing honeycomb with a thickness of about 60 mm and an impedance gradient structure.

[0063] Embodiment 14

[0064] The only difference from Example 1 is that the thickness of the absorbing film is 0.2 mm, and accordingly, the thickness of the magnetic absorbing honeycomb after curing is about 30 mm.

[0065] Embodiment 15

[0066] The only difference from Example 1 is that in step 1, the amount of carbonyl iron powder added is 100% (i.e. 300g) of the weight of the epoxy resin, and when steps 2 and 3 are subsequently repeated, it is still increased in a gradient of 5%, and the other conditions are the same as in Example 1.

[0067] Comparative Example 1

[0068] 1500 g of YPH-160 epoxy resin and 2500 g of butanone were dissolved, and 750 g of carbonyl iron powder with an average particle size of 5 microns (purchased from Jiangsu Tianyi Superfine Metal Powder Co., Ltd., with an average particle size of 5 μm) was added in a stirrer at 600 rpm, and stirring was continued for 30 min to mix evenly. The mixture was poured into an impregnation tank, and the aramid honeycomb (ACT2-3.2-48-30) was put into the impregnation tank for soaking, then taken out and dried. After most of the solvent evaporated, it was put into an oven and kept at 80°C for 60 min, 130°C for 120 min, and 160°C for 60 min to obtain a magnetic wave-absorbing honeycomb.

[0069] The materials prepared in the embodiment and the comparative example were respectively taken, and the reflectivity of the honeycomb in the range of 2 GHz to 18 GHz was tested using a bow field according to GJB2038A-2011. The test results are shown in Table 1.

[0070] Table 1

[0071]

[0072]

[0073] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: by mixing the hot-melt resin with the magnetic absorber to obtain an absorbing adhesive film, by impregnating the aramid paper or fiber felt with the absorbing adhesive film to make an absorbing impregnated felt, and then by processes such as gluing, laminating, stretching and curing to obtain a magnetic absorbing honeycomb. The present application does not involve the impregnation process in the honeycomb forming process, the forming process is simple and environmentally friendly, and the overall uniformity and absorbing strength of the honeycomb are improved.

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a magnetic wave-absorbing honeycomb, characterized in that: include: Step S1, heating the hot-melt resin to a molten state to obtain a molten resin; Step S2, mixing the molten resin with a magnetic wave absorbing agent to obtain a magnetic adhesive, and making the magnetic adhesive into a wave absorbing adhesive film; Step S3, impregnating the absorbing adhesive film with aramid paper or fiber felt to obtain an absorbing impregnated felt; Step S4, sequentially subjecting the absorbing impregnated felt to gluing, lamination, stretching and curing to obtain a magnetic absorbing honeycomb.

2. The preparation method according to claim 1, characterized in that: In the step S2, the weight ratio of the molten resin to the magnetic absorber is 20:1 to 1:2; Preferably, the weight ratio of the molten resin to the magnetic absorber is 19:1 to 1:

1.

3. The preparation method according to claim 2, characterized in that: The step S2 comprises: mixing N kinds of molten resins with the magnetic absorbers in different proportions to obtain N kinds of magnetic rubber materials, and making the N kinds of magnetic rubber materials into N kinds of absorbing adhesive films, correspondingly, when the lamination is performed in step S4, the N kinds of absorbing impregnated felts corresponding to the N kinds of absorbing adhesive films are arranged in order from low to high according to the content of the magnetic absorbing agent therein, and N=2-20; preferably, N=10~15; Preferably, after the N kinds of magnetic adhesives are arranged in ascending order according to the content of the magnetic absorber, the content of the magnetic absorber in two adjacent magnetic adhesives differs by 3-5wt%.

4. The preparation method according to any one of claims 1 or 3, characterized in that The hot-melt resin is any one or more of hot-melt epoxy resin and bismaleimide resin; Preferably, the viscosity of the hot-melt resin at 70° C. is 7000-16000 mPa·s, preferably 14000-16000 mPa·s.

5. The preparation method according to any one of claims 1 or 3, characterized in that: The magnetic wave absorbing agent includes any one or more of carbonyl iron powder, sendust aluminum alloy powder and ferrite, Preferably, the average particle size of the Sendust aluminum alloy powder is 10-13 μm. Preferably, the average particle size of the carbonyl iron powder is 5-10 μm. Preferably, the average particle size of the ferrite is 1 to 5 μm.

6. The preparation method according to any one of claims 1 or 3, characterized in that: The thickness of the wave-absorbing film is 0.1-0.2 mm.

7. The preparation method according to any one of claims 1 or 3, characterized in that: The step S3 comprises: impregnating the absorbing adhesive film with aramid paper or fiber felt to obtain an absorbing prepreg felt, and heat-keeping the absorbing prepreg felt at 80 to 90° C. for 60 to 70 minutes to obtain an absorbing feed felt; Preferably, the impregnation is single-sided impregnation.

8. The preparation method according to any one of claims 1 or 3, characterized in that: The fiber felt is aramid fiber felt.

9. The preparation method according to any one of claims 1 or 3, wherein the curing temperature is 80 to 160°C. Preferably, the curing comprises: Keep warm at 80-85°C for 55-60 min, at 125-130°C for 120-125 min, and at 155-160°C for 60-65 min.

10. A magnetic wave-absorbing honeycomb, characterized in that: The product is prepared by the preparation method described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Wave-absorbing honeycomb and manufacturing method thereof

    CN109796624A

  • Wave-absorbing honeycomb with aramid paper surface layer coated with absorbent and preparation method of wave-absorbing honeycomb

    CN115821642A

  • Acoustic board

    EP2410099A2

  • Radiowave absorber

    JP2010157696A