High-temperature-resistant vertical gold intelligent card and manufacturing method and application thereof

The pre-lamination process is used to fuse the gold-plated logo with high-temperature-resistant printing materials, which solves the problems of bubbles and unevenness during the hot-pressing fusion process of high-temperature-resistant smart cards, achieving high-temperature resistance, intelligence and unique appearance. Wenlijin smart card meets the needs of new energy vehicles.

CN118722050AActive Publication Date: 2024-10-01BEIJING HUAHONG INTEGRATED CIRCUIT DESIGN
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202410791711.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-01
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

In the existing technology, it is difficult for high-temperature-resistant smart cards to completely fuse the metal elements with the printing materials during the hot-pressing fusion process, resulting in problems such as internal bubbles, uneven surfaces, or damage to the laminated steel plates, which cannot meet the requirements of new energy vehicles for high-temperature resistance and smart cards. The need for sex and unique appearance.

Method used

Using the pre-lamination process, the gold-plated label is pasted on the printing material, and with the help of coated paper and pre-laminated steel plates, part of the thickness of the gold-plated label is sunk into the printing material through preheating and pre-cold pressing, reducing the The difficulty of lamination ensures the fusion of Lijin elements and high temperature-resistant printing materials, and forms a flat smart card under hot and cold pressing conditions.

Benefits of technology

The high-temperature-resistant Lijin smart card has no bubbles inside and a smooth surface, extending the service life and avoiding damage to the laminated steel plate. It meets the requirements of high temperature resistance, intelligence and unique appearance, and the temperature shock test shows that the card can withstand extreme temperatures. There is no obvious deformation below.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118722050A_ABST
    Figure CN118722050A_ABST
Patent Text Reader

Abstract

The invention relates to a high-temperature-resistant vertical gold intelligent card and a manufacturing method and application thereof, belongs to the technical field of intelligent card preparation, and solves the problem that in an existing intelligent card preparation method, a high-temperature-resistant material and a vertical gold material cannot be completely fused into a whole through hot pressing, and the manufacturing cost is low. The problem that bubbles appear in the high-temperature-resistant intelligent card containing the vertical gold element, the surface is uneven or the laminated steel plate is damaged is solved. The method comprises the following steps: pre-binding coated paper on a printing material pasted with a vertical gold mark, and respectively placing pre-laminated steel plates on the coated paper and the lower surface of the printing material; pre-laminating to enable the thickness of the vertical gold mark part to sink into the printing material; and binding the front surface protective film, the front printing material, the INLAY layer, the back printing material and the back surface protective film to form a large material, laminating and punching. According to the method, under the condition that the protective layer presses the steel plate, effective fusion of the high-temperature-resistant material and the vertical gold mark material is achieved, and the manufactured high-temperature-resistant intelligent card is free of bubbles in the interior and smooth in surface, has the obvious three-dimensional and metal color effect and can be widely applied to new energy automobile key cards which are vigorously developed at present.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of smart cards, and in particular to a high-temperature-resistant Lijin smart card and a manufacturing method and application thereof. Background Art

[0002] At a time when new energy vehicles are developing vigorously, car key cards are favored by many car manufacturers due to their intelligence and portability. The demand for unique and technological appearance is increasing. At the same time, their daily temperature resistance in the car has also become a key indicator for assessing the product capabilities of each manufacturer.

[0003] Smart cards containing Lijin elements have a LOGO element with a surface alloy layer embedded on the printed material under the film on the surface. The Lijin elements are integrated with the card after hot lamination, and have obvious three-dimensional and metallic color effects. In order to improve the wear resistance of smart cards, the surface of the smart card after gold lamination needs to be kept flat and without protrusions. At present, smart cards containing Lijin elements need to be pressed into the Lijin logo through hot lamination when the printed material becomes softened at a certain temperature due to the Lijin process. At the same time, considering the temperature resistance of the materials of other parts of the smart card (INLAY layer, surface protection layer, etc.), the hot lamination temperature cannot be too high, within the range of 90-150℃. Therefore, with the current Lijin process, only PVC, low-temperature resistant PET or printed materials with equivalent temperature resistance can be well hot-pressed and fused with Lijin elements within this temperature range, so that the obtained smart card has no bubbles inside and a flat surface, which meets the requirements of ISO7811-1 on the flatness of smart cards.

[0004] Different from low-temperature-resistant materials, the Vicat value of the PET material currently used in high-temperature-resistant smart cards is higher than 120°C. It is difficult to completely fuse the Lijin logo with it during lamination, resulting in bubbles inside the smart card, uneven surface, or damage to the laminated steel plate during the manufacturing process, which seriously affects the preparation, service life and appearance of high-temperature-resistant cards. Although the surface hot stamping process can also give smart cards a metallic effect, its durability is greatly reduced compared to the Lijin smart card because the hot stamping process material is on the outer surface of the card product.

[0005] In view of the demand for temperature resistance, intelligence and unique appearance of car key cards in the vigorously developing new energy vehicle field, it is urgently needed to provide a high-temperature-resistant gold-containing smart card with no bubbles inside and a smooth surface, and a preparation method thereof that will not cause damage to the laminated steel plate, so as to meet the industry standards for smart card service life, temperature resistance, appearance and other aspects, overcome the problems of existing Lijin smart cards, and meet the needs of car manufacturers for preferred Lijin smart cards. Summary of the invention

[0006] In view of the above analysis, the embodiments of the present invention aim to provide a high-temperature-resistant Limetal smart card and a manufacturing method and application thereof, so as to solve at least one of the problems of bubbles appearing inside the high-temperature-resistant smart card containing Limetal elements, uneven surface or damage to the laminated steel plate due to the inability of the high-temperature-resistant material and the Limetal material to be completely integrated through hot pressing using the existing smart card preparation method.

[0007] In a first aspect, an embodiment of the present invention provides a method for manufacturing a Lijin smart card, the method comprising:

[0008] (1) Printing text and images on the front / back printed material;

[0009] (2) pasting a gold label on the printed material, wherein the gold label has a concave-convex pattern;

[0010] (3) pre-binding coated paper on the upper surface of the printed material with the gold label, and placing pre-laminated steel plates on the lower surfaces of the coated paper and the printed material, respectively, wherein the shapes and sizes of the coated paper and the pre-laminated steel plates correspond to those of the printed material;

[0011] (4) pre-lamination to make most of the thickness of the gold mark sink into the printed material, and the pre-lamination includes pre-heating pressing and pre-cooling pressing;

[0012] (5) The front surface protective film, the front printing material, the INLAY layer, the back printing material, and the back surface protective film are bound to form a large material, laminated, and cut.

[0013] Furthermore, the Vicat value of the printing material is 120-150° C. and the thickness is 0.1-0.188 mm.

[0014] Furthermore, the gram weight of the coated paper is 128-250g / m 2 .

[0015] Furthermore, the pre-laminated steel plate has a hardness of 100-400 HBW and a thickness of 0.5-1.5 mm.

[0016] Furthermore, the preheating and pressing conditions include: a first preheating and pressing for 3-6 minutes at a temperature of 70-100°C and a pressure of 30-50 bar; a second preheating and pressing for 7-10 minutes at a temperature of 70-100°C and a pressure of 40-60 bar; and the precooling and pressing conditions include: a first precooling and pressing for 8-15 minutes at a temperature of 20-30°C and a pressure of 70-90 bar.

[0017] Furthermore, the thickness of the gold mark is 0.03-0.06 mm.

[0018] Furthermore, the thickness of the surface protection film is 0.08-0.2 mm.

[0019] Furthermore, the lamination includes hot pressing and cold pressing. Specifically, the conditions of the hot pressing include: a first hot pressing for 6-15 minutes at a temperature of 145-155°C and a pressure of 70-90 bar; a second hot pressing for 7-16 minutes at a temperature of 145-155°C and a pressure of 80-110 bar; the conditions of the cold pressing include: a first cold pressing for 3-6 minutes at a temperature of 20-30°C and a pressure of 90-120 bar; a second cold pressing for 7-16 minutes at a temperature of 20-30°C and a pressure of 100-130 bar.

[0020] In a second aspect, an embodiment of the present invention provides a LiJin smart card, which is manufactured by the method described in the first aspect.

[0021] In a third aspect, an embodiment of the present invention provides an application of a LiJin smart card in a car key card, wherein the LiJin smart card is the LiJin smart card described in the second aspect.

[0022] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0023] 1. Before laminating the INLAY layer, the printed layer with the gold label, and the surface protection layer, the printed material with the gold label is pre-laminated, so that part of the thickness (50-100%) of the gold element is sunk into the printed material, and the printed material is well integrated, thereby reducing the difficulty of laminating large materials; especially for high-temperature-resistant hard printed materials with high Vicat values ​​(≥120°C), it can also prevent bubbles from appearing inside the smart card and uneven surfaces ( Figure 4 ), and can prevent the problem of damage to the laminated steel plate and / or the smart card due to the heat-resistant material being too hard during the preparation process of the high-temperature-resistant printed smart card.

[0024] 2. The present invention limits the thickness of the printed material and the gold label, which not only needs to meet the requirements of the preparation process and application environment for the card thickness, but also needs to meet the requirements of the fusion between the gold elements and the printed material after lamination, obvious three-dimensional and metallic color effects. The thickness of the printed material of the present invention is 0.1-0.188mm, and the thickness of the gold label is 0.03-0.06mm.

[0025] 3. The high temperature resistant Lijin smart card prepared by the present invention was tested by the temperature shock method. It was found that after the smart card was temperature-shocked 100 times in the temperature range of (-35)-85°C, the card surface did not change and could be used normally. Under the same test conditions, after the low temperature resistant Lijin smart card in the prior art was temperature-shocked 100 times in the temperature range of (-35)-85°C, visible bending deformation appeared on the card surface. After the high temperature resistant Lijin smart card in the prior art was temperature-shocked 100 times in the temperature range of (-35)-85°C, the card surface had visible warping at the four corners.

[0026] 4. The coated paper used in the pre-lamination process of the present invention can be reused many times, which is energy-saving and environmentally friendly.

[0027] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0029] Figure 1 The process flow of making a high temperature resistant Lijin smart card according to the present invention;

[0030] Figure 2 This is a schematic diagram of the structure of the high temperature resistant Lijin smart card of the present invention;

[0031] Figure 3 A physical picture of a high temperature resistant Lijin smart card 1-4 made in Example 1-4 of the present invention;

[0032] Figure 4 This is a physical picture of the high temperature resistant Lijin smart card 5 prepared in Comparative Example 1 of the present invention;

[0033] Figure 5 This is a physical picture of the high temperature resistant Lijin smart card 6 prepared in comparative example 2 of the present invention;

[0034] Reference numerals:

[0035] 1-INLAY layer; 2-printing layer; 3-protective film layer; 4-gold layer. DETAILED DESCRIPTION

[0036] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0037] A specific embodiment of the present invention discloses a method for making a Lijin smart card, the method comprising:

[0038] (1) Printing text and images on the front / back printed material;

[0039] (2) pasting a gold label on the printed material, wherein the gold label has a concave-convex pattern;

[0040] (3) pre-binding coated paper on the upper surface of the printed material with the gold label, and placing pre-laminated steel plates on the lower surfaces of the coated paper and the printed material, respectively, wherein the shapes and sizes of the coated paper and the pre-laminated steel plates correspond to those of the printed material;

[0041] (4) pre-lamination to make most of the thickness of the gold mark sink into the printed material, and the pre-lamination includes pre-heating pressing and pre-cooling pressing;

[0042] (5) The front surface protective film, the front printing material, the INLAY layer, the back printing material, and the back surface protective film are bound to form a large material, laminated, and cut.

[0043] The smart card containing Lijin elements and with a smooth surface is made by pressing the Lijin mark into the printed material when it is softened at a certain temperature. At the same time, considering the temperature resistance of the materials of other parts of the smart card (INLAY layer, surface protection layer, etc.), the hot lamination temperature cannot be too high, within the range of 90-150°C. With the current Lijin process, only PVC, low-temperature resistant PET or printed materials with equivalent temperature resistance can be well hot-pressed and fused with the Lijin elements within this temperature range, so that the obtained smart card has no bubbles inside and a smooth surface, which meets the requirements of ISO7811-1 on the flatness of smart cards.

[0044] As for smart cards using high-heat-resistant printing materials, since high-heat-resistant printing materials have a higher Vicat value and a higher hardness at the same temperature, if the previous gold-plating process is used, it will be difficult to completely fuse the gold-plating mark with the hot pressing during lamination, resulting in bubbles inside the smart card and an uneven surface. If the lamination strength is increased, the gold-plating mark will be forced into the printed layer by pressure, which may easily cause damage to the laminated steel plate and / or the smart card. If the lamination temperature is increased, the printed material will be softened to allow the gold-plating mark to be pressed in. At such a high temperature, the materials of other parts of the smart card (INLAY layer, surface protection layer, etc.) will be melted into liquid, causing deformation or defects in the smart card.

[0045] Before laminating the INLAY layer, the printing layer with the gold label, and the surface protection layer, the printing layer with the gold label is pre-laminated, so that part of the thickness of the gold element is sunk into the printing material, and the printing material is well integrated, thereby reducing the difficulty of laminating large materials; especially for high-temperature-resistant hard printing materials with high Vicat values ​​(≥120°C), it can also prevent bubbles from appearing inside the smart card and uneven surfaces ( Figure 4 ), and can prevent the problem of damage to the laminated steel plate and / or the smart card due to the heat-resistant material being too hard during the preparation process of the high-temperature-resistant printed smart card.

[0046] It should be noted that the present invention can use offset printing or silk screen printing to print graphics on the front / back printing material. According to a preferred embodiment of the present invention, the present invention uses offset printing, which specifically includes: using a CTP platemaking machine to separate colors and make plates for the pattern to be offset printed, shrinking each edge of the area where the gold label is to be pasted by 0.15mm, and using a dotted line as a positioning mark for the gold label; using a UV offset printing machine to offset print the required graphics and perform UV drying, and the ink used is UV ink.

[0047] It should be noted that the front / back printing material of the present invention can be PET (polyethylene terephthalate) or other plastics with the same Vicat value range, such as one or more of PVC (polyvinyl chloride), ABS (polyacrylonitrile-butadiene-styrene), and PC (polycarbonate). According to a preferred embodiment of the present invention, the printing material of the present invention adopts PET.

[0048] It should be noted that the present invention pre-positions and pastes the gold label on the front printed material and / or the back printed material according to the pre-printed dotted positioning line, specifically: tear off the tape protective layer at the bottom of the gold label, and use the adhesive to position it on the printed material. The tape protective layer at the top of the gold label is not torn off first, and is torn off before the printed material, surface protection film, and INLAY layer are subsequently bound and positioned, which helps to make the surface of the gold label more resistant to friction before lamination.

[0049] It should be noted that the gold label of the present invention has a concave-convex pattern, which not only embeds part of the thickness of the pattern into the printing layer and integrates it with the card to increase durability, but also the pattern has obvious three-dimensional and metallic color effects.

[0050] It should be noted that the upper surface of the printed material with the gold mark is pre-bound with coated paper, and the position is aligned. For the convenience of subsequent separation, no hot binding is required. The rigidity of coated paper can press the gold mark into the high temperature resistant printed material under specific lamination parameters. At the same time, coated paper has a certain plasticity and can be reused many times, which is energy-saving and environmentally friendly.

[0051] It should be noted that a laminated steel plate is placed on the pre-bound coated paper and on the lower surface of the printed material respectively; wherein, in order to achieve a better pre-lamination effect, the shapes and sizes of the coated paper and the pre-laminated steel plate correspond to the printed material.

[0052] It should be noted that in order to embed part of the thickness of the pattern into the printed layer and integrate them into one, reduce the difficulty of laminating large smart card materials, improve the gold-plating effect of high-temperature resistant gold-plating smart cards, and reduce damage to laminated steel plates and / or smart cards, the present invention pre-laminates the gold-plating mark and printed materials.

[0053] Specifically, the pre-lamination includes hot pressing and cold pressing. During hot pressing, the printed material is in a softened state, so that most of the thickness (50-100%) of the gold mark is pressed into the printed material layer; during cold pressing, the printed material is solidified and integrated with the printed material, and the concave and convex pattern of the gold mark is higher than the printed material (but the thickness of the gold mark above the printed material is less than the thickness of the surface protective film), so that the gold mark has obvious three-dimensional and metallic color effects on the surface of the smart card, while ensuring that the surface of the smart card is flat, without protrusions, and wear-resistant.

[0054] It should be noted that the front surface protective film, front printing material, INLAY layer, back printing material, and back surface protective film are bound in order to form a large material, and then laminated and cut to make a Lijin smart card. According to specific needs, the appearance of the smart card can be further improved, such as hot stamping, varnishing, etc.; the electrical performance of the card after cutting is fully inspected; according to customer needs, the small card is personalized using a personalization device and then packaged and stored.

[0055] It should be noted that the front / back surface protective film of the present invention can be PVC, PET, PC (polycarbonate), etc. According to a preferred embodiment of the present invention, the present invention adopts a PVC surface protective film.

[0056] It should be noted that the INLAY layer of the present invention is the INLAY layer conventionally used in smart cards, which can be purchased or manufactured by any existing method.

[0057] Specifically, the preparation method of the INLAY layer comprises the following steps:

[0058] S1: Gun positioning hole

[0059] Inlay large sheet material cutting positioning holes (2), one on each adjacent side, used for positioning between subsequent large sheets, in principle, consistent with the positioning edge when cutting large materials;

[0060] S2: Module cutting and gun positioning large and small holes

[0061] Use module slitting and slitting the rolled non-contact modules, and use a specific hole punching mold to punch large and small positioning holes corresponding to the non-contact modules in the large-hole PVC layer and the small-hole PVC layer according to the antenna design drawing;

[0062] S3: Winding

[0063] The winding layer PVC is processed for wire embedding by ultrasonic winding equipment;

[0064] S4: Module positioning

[0065] The module swinging equipment uses the positioning holes of different sizes cut by the gun and the tape strips to position the non-connected modules.

[0066] S5: Module welding

[0067] Use ultrasonic welding equipment to weld the implanted enameled wire and non-contact modules.

[0068] S6: Binding

[0069] The buried wire layer, positioning layer (large hole, small hole layer) and substrate layer are bound and positioned by a binding machine.

[0070] S7: Overlay and lamination

[0071] The bound Inlay materials are laid out with high-temperature cloth, steel plate and laminating pad. Generally, 10 sets form a layer and are placed in the laminating equipment for lamination.

[0072] S8: Non-contact function detection

[0073] Use the laminated INLAY layer to carry out electrical performance test on the non-contact performance test equipment.

[0074] The Vicat value of the printed material of the present invention is 120-150°C. If the Vicat value is too low, during the manufacturing process of the Lijin smart card, it is not necessary to pre-laminate the Lijin logo and the printed layer. The printed layer with the Lijin logo, the INLAY layer and the surface protection film layer can be directly hot-laminated to well integrate the Lijin logo and the printed layer. However, the temperature resistance of the obtained smart card is very poor. If the Vicat value is too high, the Lijin logo cannot be pressed in even by the pre-lamination method of the present invention.

[0075] The thickness of the printing layer of the present invention is 0.1-0.188mm, which not only meets the requirements of the preparation process and application environment for the card thickness, but also meets the requirements that the thickness of the gold mark after lamination is partially sunken into the upper surface layer of the printing material to achieve hot pressing fusion.

[0076] It should be noted that in order to achieve the best lamination effect and take into account the economy of the material, the hardness and thickness of the coated paper need to be limited.

[0077] Specifically, the gram weight of the coated paper of the present invention is 128-250g / m 2 If the grammage of coated paper is too low, it will make it impossible to press the metallization material into the printed material, or it will make it impossible to effectively protect the laminated steel plate from being damaged by the metallization material during the lamination process; if the grammage of coated paper is too high, it will reduce the economic efficiency. First, it is unnecessary in terms of technology and wastes resources. Second, when the grammage is too high, lamination will leave a mark of the metallization mark on the coated paper, which cannot be reused and causes waste.

[0078] It should be noted that in order to ensure a better pre-lamination effect, the thickness and hardness of the pre-laminated steel plate need to be limited.

[0079] Specifically, the hardness of the pre-laminated steel sheet of the present invention is 100-400 HBW, and the thickness ranges from 0.5-1.5 mm. If the hardness of the pre-laminated steel sheet is too small, the pre-laminated steel sheet is easily scratched and dented; and if the hardness of the pre-laminated steel sheet is too large, the production cost is too high. If the thickness of the pre-laminated steel sheet is too small, it is easy to deform during the pre-lamination process, and if the thickness is too large, the cost will increase.

[0080] It should be noted that in order to achieve the fusion between the printed material and the gold label, the present invention needs to preheat and press the printed material with the gold label.

[0081] Specifically, the conditions of the preheating and pressing include: a primary preheating and pressing for 3-6 minutes at a temperature of 70-100°C and a pressure of 30-50 bar; a secondary preheating and pressing for 7-10 minutes at a temperature of 70-100°C and a pressure of 40-60 bar; through segmented preheating and pressing, the air between the card materials can be discharged through the gradual pressurization process, which is also beneficial to the protection of the INLAY layer chip in the card. The appropriate temperature puts the printed material in a suitable softening state to press the gold mark, and avoids the printing material from being transformed into a liquid phase due to too high a temperature; the appropriate pressure ensures that the gold mark is partially pressed into the softened printed material, and avoids the gold mark being completely pressed into the printed material, causing the gold mark to lose its three-dimensional and metallic color effect on the smart card. If the hot pressing time is too short, the gold mark cannot be well integrated with the printed material; if the time is too long, it will cause a waste of production capacity resources.

[0082] It should be noted that in order to solidify the shape of the printed layer and the gold mark after lamination, the present invention needs to pre-cold press the printed material with the gold mark attached after pre-heating and pressing.

[0083] Specifically, the conditions of the pre-cold pressing include: 8-15 minutes of pre-cold pressing at a temperature of 20-30°C and a pressure of 70-90 bar. If the cold pressing temperature is too high, the morphology of the printed layer after pre-lamination cannot be solidified; if the temperature is too low, sudden cooling after heating is likely to cause deterioration and brittleness of the card material and adverse phenomena caused by water vapor generation. Excessive cold pressing pressure will cause damage to the printed layer or the gold label, and too little pressure will make it impossible to obtain the final laminated morphology of the printed layer and the gold label. If the cold pressing time is too long, energy will be wasted; if the time is too short, it will not be possible to completely solidify, cool and obtain the final state after pre-lamination.

[0084] It should be noted that in order to allow part of the thickness of the gold mark to be integrated with the printed material through pre-lamination, while ensuring that the gold mark has obvious three-dimensional and metallic color on the smart card and has a certain amount of economic rationality, the present invention needs to limit the thickness of the gold mark.

[0085] Specifically, the thickness of the gold label is 0.03-0.06 mm. If the gold label is too thick, it is easy for the gold label to penetrate the printed layer during pre-lamination, or the thickness of the part of the gold label protruding from the printed plane is too thick, resulting in failure in the subsequent smart card manufacturing or bubbles and uneven surface of the gold label; if the gold label is too thin, the three-dimensional effect is not obvious.

[0086] It should be noted that in order to allow the surface protection film to fuse and cover the portion of the gold mark protruding from the printed material during the lamination process of the smart card, the thickness of the surface protection film layer of the smart card needs to be limited.

[0087] Specifically, the thickness of the surface protection film is 0.08-0.2 mm. If the surface protection film is too thick, the thickness of the smart card cannot meet the requirements of the card manufacturing process and the use environment; if the surface protection film is too thin, the gold mark cannot be well fused and coated, and the gold mark is easy to fall off.

[0088] It should be noted that in order to combine the printed material with the Lijin mark, the INLAY layer, and the surface protection film to form a Lijin smart card, and at the same time fuse and cover the part of the Lijin mark protruding from the printed material with the surface protection film, it is necessary to laminate the layers of the smart card. Specifically, before lamination, the layers need to be bound in the order of front surface protection film, front printed material, INLAY layer, back printed material, and back surface protection film to form a large material, wherein the front printed material and / or back printed material of the large material are fused with the Lijin mark.

[0089] Specifically, the lamination includes hot pressing and cold pressing. Specifically, the conditions of the hot pressing include: a first hot pressing for 6-15 minutes at a temperature of 145-155°C and a pressure of 70-90 bar; a second hot pressing for 7-16 minutes at a temperature of 145-155°C and a pressure of 80-110 bar; the conditions of the cold pressing include: a first cold pressing for 3-6 minutes at a temperature of 20-30°C and a pressure of 90-120 bar; a second cold pressing for 7-16 minutes at a temperature of 20-30°C and a pressure of 100-130 bar. Segmented hot lamination and segmented cold lamination are beneficial to the discharge of gas inside the card during the lamination process, which is beneficial to improving the lamination yield rate; the smart card material is softened at a suitable temperature and forms a tight bond under the action of suitable pressure. The lamination temperature and pressure are interrelated. Appropriate temperature and pressure help to improve the bonding effect, strength and appearance of the smart card; in addition, the lamination time is also very important. If the hot lamination time is too short, it will affect the bonding effect and strength of the card; if the hot lamination time is too long, it will cause defects such as deformation, wrinkles or discoloration on the surface of the card, affecting the appearance of the card and increasing the production cycle and cost.

[0090] It should be noted that during the lamination, a laminating pad needs to be placed between the upper and lower surfaces of the bulk material and the laminating steel plate, and the material of the laminating pad is silica gel or felt. According to a preferred embodiment of the present invention, multiple layers of bulk material can be stacked during lamination, and the laminating steel plate is placed on the upper and lower surfaces of each layer of bulk material, and a laminating pad is placed between the uppermost and lowermost laminating plates and the bulk material of each layer of bulk material in the laminating machine, and the multiple layers are 2-10 layers.

[0091] A specific embodiment of the present invention discloses a smart card, such as Figure 2 , 3 As shown, the LiJin smart card is manufactured by the method described in the first aspect.

[0092] The high temperature resistant Lijin smart card prepared by the method of the present invention was tested by the temperature shock method. It was found that after the smart card was temperature-shocked 100 times in the temperature range of (-35)-85°C, the card surface did not change and could be used normally; under the same test conditions, after the low temperature resistant Lijin smart card in the prior art was temperature-shocked 100 times in the temperature range of (-35)-85°C, visible bending deformation appeared on the card surface; after the high temperature resistant Lijin smart card in the prior art was temperature-shocked 100 times in the temperature range of (-35)-85°C, the card surface had visible four corners warping.

[0093] A specific embodiment of the present invention discloses an application of a LiJin smart card in a car key card, wherein the LiJin smart card is the LiJin smart card described in the second aspect.

[0094] The smart card containing the Li-metal element of the present invention is applied to a car key card, which is not only easy to carry, but also has a unique and technological appearance and is durable.

[0095] Example 1

[0096] A method for making a gold-labeled smart card 1, the method comprising:

[0097] (1) Use a UV offset printing machine to offset print a gold mark on the PET positive printing material. The Vicat value of the printing material is 120°C and the thickness is 0.188 mm.

[0098] (2) tearing off the protective tape layer at the bottom of the gold label, and pasting the gold label showing the words "Beijing Huahong" and the logo on the preset area on the positive printed material in step (1), wherein the gold label has a concave-convex pattern and a thickness of 0.04 mm;

[0099] (3) Coated paper is pasted on the upper surface of the positive printed material with the gold label, and pre-laminated steel plates are placed on the upper surface of the coated paper and the lower surface of the positive printed material, respectively. The gram weight of the coated paper is 200g / m 2 ; The hardness of the pre-laminated coated paper is 300 HBW and the thickness is 0.8 mm; The size of the coated paper and the pre-laminated steel plate is comparable to that of the PET positive printing material;

[0100] (4) Pre-lamination, specifically: pre-heating and pressing for 5 minutes at a temperature of 90° C. and a pressure of 40 bar; pre-heating and pressing for 8 minutes at a temperature of 90° C. and a pressure of 50 bar; pre-cooling and pressing for 10 minutes at a temperature of 20° C. and a pressure of 80 bar, to obtain a positive printing material with a gold mark fused on the surface layer;

[0101] (5) The PVC front surface protection film, the front printing material obtained in step (4), the INLAY layer, the PET back printing material, and the PVC back surface protection film are sequentially stacked, positioned, and bound to form a large material; 10 layers of the large material are stacked, and the laminating steel plates are placed on the upper and lower surfaces of the 10 layers of the large material, respectively, and a silicone laminating pad is set between the uppermost and lowermost laminating steel plates and the large material every 10 layers of the large material on the laminating machine; lamination, specifically: hot pressing for 10 minutes at a temperature of 150°C and a pressure of 80 bar; hot pressing for 15 minutes at a temperature of 150°C and a pressure of 90 bar; cold pressing for 5 minutes at a temperature of 20°C and a pressure of 100 bar; cold pressing for 10 minutes at a temperature of 20°C and a pressure of 120 bar to form a large sheet, and cutting it to obtain the Lijinbiao smart card 1.

[0102] Photos showing the Lijin Label Smart Card 1 Lijin effect Figure 3 As shown (left), from Figure 3It can be seen that there are no bubbles inside the Lijin smart card 1, the surface is flat, and it has obvious three-dimensional and metallic color effects. The Lijin smart card 1 was tested using the temperature shock method and it was found that after the smart card was subjected to temperature shock 100 times in the temperature range of (-35)-85℃, there was no warping on the card surface and it can be used normally.

[0103] Example 2

[0104] A gold-labeled smart card 2 was prepared according to the preparation method of Example 1, except that the thickness of the PET positive printing material was 0.1 mm.

[0105] Photos showing the Lijin effect of Lijin Biao Smart Card 2 Figure 3 As shown (second from left), Figure 3 It can be seen that there are no bubbles inside the Lijinbiao smart card 2, the surface is flat, and it has obvious three-dimensional and metallic color effects. The Lijin smart card 2 was tested using the temperature shock method and it was found that after the smart card was subjected to temperature shock 100 times in the temperature range of (-35)-85℃, there was no warping on the card surface and it can be used normally.

[0106] Example 3

[0107] The Lijin Label smart card 3 was prepared according to the preparation method of Example 1, except that the weight of the coated paper used for pre-lamination was 158 g / m 2 .

[0108] Photos showing the Lijin effect of Lijin Biao Smart Card 3 Figure 3 As shown (third from left), Figure 3 It can be seen that there are no bubbles inside the Lijinbiao smart card 3, the surface is flat, and it has obvious three-dimensional and metallic color effects. The Lijin smart card 3 was tested using the temperature shock method and it was found that after the smart card was subjected to temperature shock 100 times in the temperature range of (-35)-85℃, there was no warping on the card surface and it can be used normally.

[0109] Example 4

[0110] The Lijinbiao smart card 4 was prepared according to the preparation method of Example 1, except that the pre-lamination process was: preheating and pressing for 5 minutes at a temperature of 100°C and a pressure of 30 bar; preheating and pressing for 8 minutes at a temperature of 100°C and a pressure of 40 bar; and precooling and pressing for 10 minutes at a temperature of 30°C and a pressure of 80 bar.

[0111] Photos showing the Lijin effect of Lijin Biao smart card 4 Figure 3 As shown (fourth from left), Figure 3It can be seen that there are no bubbles inside the Lijinbiao smart card 4, the surface is flat, and it has obvious three-dimensional and metallic color effects. The Lijin smart card 4 was tested using the temperature shock method and it was found that after the smart card was subjected to temperature shock 100 times in the temperature range of (-35)-85℃, there was no warping on the card surface and it can be used normally.

[0112] Comparative Example 1

[0113] The method for making the gold-labeled smart card 5 is the same as the method for making the smart card in Example 1, except that the method for making the gold-labeled smart card 5 does not include steps (3) and (4) of pre-laminating the positive printed material with the gold-labeled smart card using coated paper and pre-laminated copper plate.

[0114] Photos showing the Lijin effect of Lijin smart card 5 Figure 4 As shown, from Figure 4 It can be seen that there are bubbles inside the Lijinbiao smart card 5 and the surface is uneven. After the Lijinbiao smart card 5 is subjected to temperature shock for 100 times in the temperature range of (-35)-85℃, the four corners of the card surface will be visibly lifted.

[0115] Comparative Example 2

[0116] The method for making the gold-labeled smart card 6 is the same as that of the embodiment 1, except that:

[0117] The PET positive printing material was replaced with PC positive electrode material with a Vicat value of 160°C.

[0118] Photos showing the Lijin Label Smart Card 6 Lijin effect Figure 5 As shown, from Figure 5 It can be seen that there are bubbles inside the LiJinBiao smart card 6 and the surface is uneven.

[0119] Comparative Example 3

[0120] The method for making the Lijinbiao smart card 7 is the same as the method for making the embodiment 1, except that the weight of the coated paper is 60 g / m 2 It was found that the pre-laminated steel sheets were damaged during the preparation of the smart card.

[0121] Comparative Example 4

[0122] The same method as in Example 1 was used, except that the pre-lamination in step (4) only included a pre-heating pressing process but not a pre-cooling pressing process. It was found that the printed material after being fused with the gold mark was bent during the subsequent cooling process.

[0123] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for making a Lijin smart card, characterized in that: The method comprises: (1) Printing text and images on the front / back printed material; (2) pasting a gold label on the printed material, wherein the gold label has a concave-convex pattern; (3) pre-binding coated paper on the upper surface of the printed material with the gold label, and placing pre-laminated steel plates on the lower surfaces of the coated paper and the printed material, respectively, wherein the shapes and sizes of the coated paper and the pre-laminated steel plates correspond to those of the printed material; (4) pre-lamination to make most of the thickness of the gold mark sink into the printed material, and the pre-lamination includes pre-heating pressing and pre-cooling pressing; (5) The front surface protective film, the front printed material, the INLAY layer, the back printed material, and the back surface protective film are bound together to form a large material, laminated, and cut.

2. The method according to claim 1, characterized in that The printing material has a Vicat value of 120-150° C. and a thickness of 0.1-0.188 mm.

3. The method according to claim 1, characterized in that The gram weight of the coated paper is 128-250g / m 2 .

4. The method according to claim 1, characterized in that: The hardness of the pre-laminated steel plate is 100-400 HBW and the thickness is 0.5-1.5 mm.

5. The method according to claim 1, characterized in that The preheating and pressing conditions include: a first preheating and pressing for 3-6 minutes at a temperature of 70-100°C and a pressure of 30-50 bar; a second preheating and pressing for 7-10 minutes at a temperature of 70-100°C and a pressure of 40-60 bar; the precooling and pressing conditions include: a precooling and pressing for 8-15 minutes at a temperature of 20-30°C and a pressure of 70-90 bar.

6. The method according to claim 1, characterized in that The thickness of the gold mark is 0.03-0.06 mm.

7. The method according to claim 1, characterized in that The thickness of the surface protection film is 0.08-0.2 mm.

8. The method according to claims 1-7, characterized in that The lamination includes hot pressing and cold pressing. The conditions of the hot pressing include: a first hot pressing for 6-15 minutes at a temperature of 145-155°C and a pressure of 70-90 bar; a second hot pressing for 7-16 minutes at a temperature of 145-155°C and a pressure of 80-110 bar; the conditions of the cold pressing include: a first cold pressing for 3-6 minutes at a temperature of 20-30°C and a pressure of 90-120 bar; a second cold pressing for 7-16 minutes at a temperature of 20-30°C and a pressure of 100-130 bar.

9. A LiJin smart card, characterized in that: The LiJin smart card is manufactured by the method described in any one of claims 1-8.

10. An application of Lijin smart card in car key card, characterized in that: The LiJin smart card is the LiJin smart card described in claim 9.

Citation Information

Patent Citations

  • Device and method for nondestructively recycling chips

    CN101856664A

  • Makrolon / modified polyester blending rolling base material and preparation method thereof

    CN101864161A

  • Laminating method

    CN105917511A

  • Intelligent card with metal luster and preparation method of intelligent card

    CN107085740A

  • Forming method of double-faced complex cavity of multilayer ceramic substrate

    CN107214828A