Method for preparing battery-grade iron phosphate by taking high-pressure hydrolysate of cobalt-iron alloy pickle liquor as raw material
By reacting the high-pressure hydrolyzate of cobalt-iron alloy acid leaching solution with phosphoric acid, combined with pH control and oxidation treatment, battery-grade iron phosphate was successfully prepared, solving the problem of resource utilization and high production cost, and realizing high-efficiency and low-cost batteries. Preparation of grade iron phosphate.
Patent Information
- Application Number
- CN202410949087.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-16
AI Technical Summary
It is difficult to effectively utilize the high-pressure hydrolyzate of cobalt-iron alloy acid leaching solution to prepare battery-grade iron phosphate with the existing technology, resulting in resource utilization difficulties and high production costs.
By mixing the high-pressure hydrolyzate powder of the cobalt-iron alloy acid leaching liquid with the phosphoric acid solution, and after heating the reaction, the pH value of the solution is controlled, reduced iron powder and H2O2 are added, and the pH value is adjusted to precipitate to obtain the battery-grade iron phosphate FePO4 product.
It achieves efficient utilization of cobalt-iron alloy acid leaching liquid resources, reduces production costs, improves the purity and iron-phosphorus ratio of battery-grade iron phosphate, simplifies the washing process, and is suitable for large-scale production.
Smart Images

Figure CN118723958A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource utilization of cobalt-iron alloy acid leaching solution and preparation of battery-grade iron phosphate, and relates to a method for preparing battery-grade iron phosphate by using a high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution as a raw material. Background Art
[0002] Lithium iron phosphate (LiFePO 4 ) has the characteristics of high energy density, excellent cycle stability and safety stability, and is an excellent positive electrode material for lithium-ion batteries. Due to its own structural stability, lithium iron phosphate can maintain a relatively stable structure even at high temperatures, and even when the battery is deformed and damaged, it will not cause safety accidents such as smoke and fire. The thermal decomposition temperature of fully charged lithium iron phosphate material is about 700°C, while the thermal decomposition temperature of ternary materials is 200-300°C, making lithium iron phosphate batteries very safe and reliable. In recent years, due to the rapid increase in market demand for lithium iron phosphate, the demand for battery-grade iron phosphate, the precursor of lithium iron phosphate, has also increased sharply. Traditional battery-grade iron phosphate is prepared by reacting iron sheet with phosphoric acid, but there are: (1) the cost of iron sheet, which increases the cost of preparing iron phosphate; (2) the reaction of iron sheet with phosphoric acid will release a large amount of dangerous gas hydrogen. These two problems limit the large-scale production of iron phosphate. In recent years, the preparation of battery-grade iron phosphate by iron-containing waste liquid has become a hot topic in the industry. First, iron-containing waste liquid has basically no cost, and enterprises can use iron-containing waste liquid as raw material to replace iron sheets, thereby reducing the cost of iron sheets. Second, the reaction of iron-containing waste liquid does not involve the production of dangerous hydrogen, thus bringing safety protection to enterprise production.
[0003] Cobalt-iron alloys are mainly derived from cobalt-containing slags in copper smelting. Cobalt-iron alloys contain a large amount of iron and a small amount of cobalt. After the cobalt-iron alloy is treated with sulfuric acid leaching, a small amount of cobalt is extracted by adjusting the reaction process parameters, while a large amount of iron exists in the liquid phase solution. Iron mainly exists in the form of ferrous sulfate in the solution. The hydrolysis of iron ions is the most important and common reaction for precipitation and separation of iron. It is also a very complicated process. The properties of the solution and the hydrolysis conditions have an important influence on the results of the hydrolysis. The hydrolysis compositions and structures of different outputs are different. A lot of research has been done on the reaction mechanism of the high-temperature hydrolysis products of ferrous sulfate solutions (mainly iron oxides and hydroxides). The process of hydrolysis of ferrous sulfate to form a precipitate is a high-temperature oxidation hydrolysis precipitation, and because the solubility of ferrous sulfate is low under high temperature conditions, the precipitation process is accompanied by the re-dissolution process of ferrous sulfate. How to use the high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution to prepare battery-grade iron phosphate has become an important research topic, and it is also a research hotspot and difficulty in the current industry.
[0004] With the rapid development of my country's new energy industry, battery manufacturers have to take into account the cost, difficulty of process control and performance, and the supply of battery-grade iron phosphate raw materials and environmental protection issues are becoming increasingly prominent. In this context, seeking alternative raw materials and resource utilization of iron-containing waste liquid / waste solid has become the focus of industry attention. For example, CN202011436682.2 provides a method for preparing battery-grade flaky iron phosphate using cobalt-iron leachate. However, no literature reports have been found on the preparation of battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing battery-grade ferric phosphate using the high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution as a raw material, thereby solving the problem of resource utilization of iron elements in the high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution, and finally obtaining high-value-added battery-grade ferric phosphate products.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A method for preparing battery-grade iron phosphate using a high-pressure hydrolysis product of a cobalt-iron alloy acid leaching solution as a raw material comprises the following steps:
[0008] (1) adding powder of high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution into deionized water, mixing and stirring, then adding phosphoric acid solution, stirring evenly to obtain a yellow mixed solution, heating for reaction, filtering to obtain a clear solution, and controlling the pH value of the solution to be 1.10-1.20;
[0009] (2) Add reduced iron powder to the obtained clear solution while stirring, and then add H 2 O 2 , continue stirring, and then filter;
[0010] (3) adjusting the pH value of the solution obtained after filtering in step (2) to between 2.85 and 3.50 to obtain a white precipitate, filtering, washing, and drying the precipitate to obtain battery-grade iron phosphate FePO 4 product.
[0011] Furthermore, in step (1), the concentration of the phosphoric acid solution is 35-45 wt %.
[0012] Furthermore, in step (1), the heating reaction temperature is 100-110° C. and the time is 1-3 h.
[0013] Furthermore, in step (1), the heating reaction temperature is 105° C. and the time is 2 h.
[0014] Furthermore, in step (2), the amount of reduced iron powder added is about 4 times the mass of the powder of the high-pressure hydrolysis product of the cobalt-iron alloy acid leaching solution, and the reduced iron powder consumes excess phosphoric acid, and the pH value of the solution is between 1.50 and 1.70.
[0015] Furthermore, in step (2), H 2 O 2 The amount is 50-70% by weight of the powder of the high-pressure hydrolysis product of the cobalt-iron alloy acid leaching solution, and can be 60% by weight, and the concentration is 25-35wt%.
[0016] Furthermore, in step (2), the stirring time is continued for 50-70 minutes, and the stirring temperature is room temperature.
[0017] Furthermore, in step (3), the reagent used to adjust the pH value is aqueous ammonia.
[0018] Furthermore, in step (3), the concentration of the ammonia water is 8-12 wt %. Exemplarily, the concentration of the ammonia water is 10 wt %.
[0019] The prior art generally uses mixed acid to dissolve cobalt concentrate or cobalt alloy. On the one hand, it consumes acid (sulfuric acid, hydrochloric acid and nitric acid, etc.) with a certain cost. On the other hand, when the pH value of the solution is adjusted, the residual mixed acid will increase the amount of alkaline regulator, thereby increasing the cost of preparing battery-grade iron phosphate. The present invention directly uses phosphoric acid to react with the high-pressure hydrolysis product of cobalt-iron acid leaching liquid to prepare battery-grade iron phosphate, thereby reducing the cost of using the regulator in the pH adjustment process, and can avoid the introduction of impurity anions such as sulfate and chloride ions into the reaction system during the mixed acid dissolution process. These impurity anions are more difficult in the final battery-grade iron phosphate product washing process. There are many impurity elements (Al, Si and Ca, etc.) in cobalt concentrate or cobalt alloy, and battery-grade iron phosphate products require impurity elements at the ppm level, with a high technical threshold, requiring very effective impurity removal technology methods, and the cost of preparing battery-grade iron phosphate needs to be comprehensively considered. The present invention directly uses the high-pressure hydrolysis product of cobalt-iron alloy acid leaching liquid to react with phosphoric acid to prepare battery-grade iron phosphate, which can not only effectively control the content of impurity elements, but also significantly reduce the production cost during the reaction process, and effectively reduce the difficulty of washing the iron phosphate product.
[0020] Since the high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution has a high content of chromium (Cr% = 0.127) and calcium (Ca% = 0.118), and the battery-grade iron phosphate requires the chromium content (Cr% ≤ 0.005) and calcium content (Ca% ≤ 0.005) to be in a relatively low range. Therefore, the preparation of battery-grade iron phosphate using the high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution as a raw material has a high technical threshold. The concept of the present invention is to first dissolve the high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution with phosphoric acid. Phosphoric acid is a medium-strength acid. The high-pressure hydrolysis product can be dissolved by appropriate heating, and the generated iron phosphate is dissolved in excess phosphoric acid. The pH value of the solution is controlled to be 1.10-1.20. At this time, the substances in the high-pressure hydrolysis product that are difficult to dissolve in phosphoric acid can be removed by filtration. Then add an appropriate amount of reduced iron powder to the purified clear and transparent solution to neutralize the excess phosphoric acid. Then add H 2 O 2 , continue stirring and filtering the solution, H 2 O 2 The divalent iron ions can be oxidized into trivalent iron ions to increase the iron-phosphorus ratio of the final battery-grade iron phosphate product. The pH value of the solution is then adjusted to between 2.85 and 3.50 with ammonia water. At this time, a large amount of white precipitate is produced. The precipitate is filtered, washed and dried to finally obtain battery-grade iron phosphate FePO 4 product.
[0021] The main feature of the present invention is to use the high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution as raw material, remove impurity elements in the high-pressure hydrolysis product through the dissolution-impurity removal-oxidation-precipitation strategy to obtain battery-grade iron phosphate FePO 4 There is no related technical report on this product.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] (1) Using the high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution as raw material, battery-grade iron phosphate FePO was prepared through the dissolution-impurity removal-oxidation-precipitation process route and the regulation of reaction conditions and parameters. 4 The product, the prepared battery-grade iron phosphate is a white powder product;
[0024] (2) Remove impurities such as calcium and chromium by controlling the pH value of the solution, and 2 O 2 Oxidation of divalent iron ions increases the iron-phosphorus ratio of ferric phosphate products. This technical method is simple and effective, and no other impurity ions are introduced during the entire process. The prepared battery-grade iron phosphate FePO 4 High product purity;
[0025] (3) The method of the present invention is applicable to the preparation of battery-grade iron phosphate products from most iron-containing waste solids. The dissolution-decontamination-oxidation-precipitation process adopted is universal, the cost of the entire reaction process is very low, and high temperature, high pressure and other treatments are not required. It has the advantages of low energy consumption and easy industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a process flow chart of the present invention;
[0027] Figure 2 This is an optical photograph of a powder sample of a high-pressure hydrolysis product of a cobalt-iron alloy acid leaching solution;
[0028] Figure 3 The battery-grade iron phosphate FePO prepared by the present invention 4 Optical photograph of the product;
[0029] Figure 4 The battery-grade iron phosphate FePO prepared by the present invention 4 XRD analysis results of the product;
[0030] Figure 5 The battery-grade iron phosphate FePO prepared by the present invention 4 Scanning electron microscope photograph of the product;
[0031] Figure 6 The battery-grade iron phosphate FePO prepared by the present invention 4 Transmission electron microscope picture of the product. DETAILED DESCRIPTION
[0032] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0033] In the following examples, unless otherwise specified, raw materials or processing techniques are conventional commercially available raw materials or conventional processing techniques in the art.
[0034] Embodiment 1:
[0035] This embodiment provides a method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials. The preparation process is as follows: Figure 1 shown.
[0036] The high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution is a yellow powder sample. The high-pressure hydrolysis product mainly comes from the cobalt-iron slag in the copper smelting process, which is enriched by reduction roasting-crushing-magnetic separation, and then obtained by dilute sulfuric acid acid leaching, high-pressure hydrolysis, separation and drying. Its optical photo is shown in Figure 2As shown, the composition analysis of the high-pressure hydrolysis product used in this embodiment is shown in Table 1. As can be seen from Table 1, the content of chromium (Cr% = 0.127) and calcium (Ca% = 0.118) in the high-pressure hydrolysis product is relatively high, which is much higher than the chromium content (Cr% ≤ 0.005) and calcium content (Ca% ≤ 0.005) in battery-grade iron phosphate. Therefore, it is necessary to remove chromium and calcium in the process of preparing battery-grade iron phosphate.
[0037] Table 1
[0038] <![CDATA[Al 2 THE 3 ]]> <![CDATA[SiO 2 ]]> <![CDATA[P 2 THE 5 ]]> <![CDATA[SO 3 ]]> CaO <![CDATA[V 2 THE 5 ]]> <![CDATA[Cr 2 THE 3 ]]> 785.6ppm 387.0ppm 0.280% 6.457% 0.118% 54.9ppm 0.127% <![CDATA[Fe 2 THE 3 ]]> NiO ZnO <![CDATA[ZrO 2 ]]> <![CDATA[MoO 3 ]]> <![CDATA[Ag 2 The]]> 85.957% 0.119% 403.2ppm 224.8ppm 9.3ppm 0.140%
[0039] In this embodiment, 1g of high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution was measured, 28g of dilute phosphoric acid solution with a concentration of 40wt% was added, and after mixing and stirring, deionized water was added to adjust the volume of the mixed solution to 200mL, and the mixture was heated to 105℃ in an oil bath pot, the reaction time was 2h, and the pH of the solution was controlled at about 1.17. Then the solution was filtered, 4g of reduced iron powder was added to the resulting solution to neutralize the excess phosphoric acid, and then 0.6g of H2O with a concentration of 30wt% was added. 2 O 2 , continue to stir and filter the solution, and then adjust the pH value to 2.85 with 10wt% ammonia solution. At this time, a large amount of white precipitate is produced in the solution. The white precipitate is filtered, washed and dried to obtain battery-grade iron phosphate FePO 4 product( Figure 3 ).
[0040] Prepared battery-grade iron phosphate FePO 4 The X-ray diffraction (XRD) analysis results of the product are as follows: Figure 4 As shown. Figure 4 It can be seen that the diffraction peak of the prepared product is similar to that of FePO 4 The composition is consistent, and the XRD diffraction peak of the product is relatively strong, indicating that the prepared battery-grade iron phosphate FePO 4 The product has good crystallinity. 4 Scanning electron microscope (SEM) photos of the product are as follows: Figure 5 As shown. Figure 5 It can be seen that the prepared FePO 4 The product is a flower-like microsphere with a size of about 20 μm. 4 The microspheres are uniform in size and have spherical structures. High-magnification SEM shows that FePO 4 The microspheres are composed of a large number of lamellar structures. 4 Transmission electron microscope (TEM) photos of the product are as follows: Figure 6 As shown. Figure 6 It can be seen that the prepared FePO4 Microspheres are composed of many lamellar structures with a length of several hundred nanometers and a thickness of tens of nanometers.
[0041] The battery-grade iron phosphate FePO prepared above 4 The inductively coupled plasma atomic emission spectroscopy (ICP) analysis of the product is shown in Table 2. As can be seen from Table 2, iron phosphate FePO 4 The calcium and chromium impurities in the product can be effectively controlled, and the contents of other impurity elements are also within the standard range of battery-grade iron phosphate, and the prepared iron phosphate product Fe:P=0.9824. Therefore, the battery-grade iron phosphate prepared by the present invention using the high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution as a raw material has high quality and has important application prospects in the field of resource utilization of iron-containing waste solids such as the high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution.
[0042] Table 2
[0043] Al% Ca% Co% Cr% Cu% K% Mg% Na% 0.0155 0.005 0.0002 0.00252 Not detected 0.0028 Not detected 0.0053 P% Ni% Fe% Mn% Ti% Zn% Pb% Fe:P ratio 17.43 0.0007 30.88 0.0052 0.0258 0.0018 Not detected 0.9824
[0044] Embodiment 2:
[0045] In this embodiment, 1g of high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution was measured, and 28g of dilute phosphoric acid solution with a concentration of 40wt% was added. After the high-pressure hydrolysis product and the dilute phosphoric acid were mixed, stirring was continued, and then deionized water was added to control the total volume of the mixture solution to 200mL, and then the mixture was heated to 105°C in an oil bath pot, and the pH of the solution was controlled to be about 1.17. The mixture reaction time was 2h. Then the solution was filtered, and 4g of reduced iron powder was added to the solution. Excess phosphoric acid would react with the reduced iron powder, and then 0.6g of H with a concentration of 30wt% was added. 2 O 2 , continue to stir the solution. After sufficient stirring and filtering, adjust the pH value to 3.50 with 10wt% ammonia solution. At this time, a large amount of white precipitate is obtained, and then the white precipitate is filtered, washed and dried to obtain battery-grade iron phosphate FePO 4 product.
[0046] Preparation of iron phosphate FePO 4 The ICP analysis of the product is shown in Table 3. As can be seen from Table 3, the prepared iron phosphate product Fe:P=0.9830, and the prepared iron phosphate product meets the requirements of battery-grade iron phosphate. When the solution pH value increases from 2.85 to 3.50, the iron ions in the solution will further precipitate, resulting in an increase in the iron-phosphorus ratio from 0.9824 to 0.9830. Therefore, the solution pH value is also an important reaction parameter for regulating the iron-phosphorus ratio in the iron phosphate product.
[0047] Table 3
[0048] Al% Ca% Co% Cr% Cu% K% Mg% Na% 0.0136 0.0049 0.0003 0.00247 Not detected 0.0021 Not detected 0.0048 P% Ni% Fe% Mn% Ti% Zn% Pb% Fe:P ratio 17.35 0.0006 30.75 0.0041 0.0223 0.0012 Not detected 0.9830
[0049] Comparative Example 1:
[0050] Compared with Example 1, most of the steps are the same except that the step of adding Fe powder is omitted.
[0051] 1g of high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution was mixed with 28g of dilute phosphoric acid solution with a concentration of 40wt%, and then deionized water was added to 200mL. The mixture was heated to 105℃ in an oil bath pot for 2h, and the pH of the solution was controlled at about 1.17. The solution was then filtered, and 0.6g of H2O with a concentration of 30wt% was directly added to the resulting solution without adding reduced iron powder. 2 O 2 , continue to stir and filter the solution, and then adjust the pH value to 2.85 with 10wt% ammonia solution. At this time, a large amount of white precipitate is produced in the solution. The white precipitate is filtered, washed and dried to obtain battery-grade iron phosphate FePO 4 product.
[0052] Preparation of iron phosphate FePO 4 The ICP analysis of the product is shown in Table 4. As can be seen from Table 4, without adding reduced iron powder, the calcium and chromium content in the ferric phosphate product is high, and the iron content in the ferric phosphate product is low, and the iron-phosphorus ratio is only 0.618, indicating that there is an excess of phosphoric acid in the reaction process, there are many by-products in the product, and a battery-grade ferric phosphate product with a high iron-phosphorus ratio cannot be obtained.
[0053] Table 4
[0054] Al% Ca% Co% Cr% Cu% K% Mg% Na% 0.004 0.018 Not detected 0.019 Not detected 0.0035 Not detected 0.0057 P% Ni% Fe% Mn% Ti% Zn% Pb% Fe:P ratio 19.341 0.0005 21.585 0.0067 0.0236 0.0023 Not detected 0.618
[0055] Comparative Example 2:
[0056] Compared with Example 1, most of the steps are the same, except that the pH value of the subsequent ammonia adjustment is changed to 3.8.
[0057] 1g of high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution was mixed with 28g of dilute phosphoric acid solution with a concentration of 40wt%. After mixing and stirring, deionized water was added to adjust the volume of the mixed solution to 200mL, and then the mixture was heated to 105℃ in an oil bath pot for 2h. The pH of the solution was controlled at about 1.17. The solution was filtered, 4g of reduced iron powder was added to the resulting solution, and then 0.6g of 30% H 2 O 2 , continue to stir and filter the solution, and then adjust the pH value to 3.80 with 10wt% ammonia solution. At this time, a large amount of white precipitate is produced in the solution. The white precipitate is filtered, washed and dried to obtain battery-grade iron phosphate FePO 4 product.
[0058] Preparation of iron phosphate FePO4 The ICP analysis of the product is shown in Table 5. As can be seen from Table 5, as the pH value of the solution increases from 3.50 to 3.80, the iron-phosphorus ratio decreases. This is because the excess ammonia water will complex with iron ions to form a water-soluble complex, thereby reducing the iron content in the precipitated iron phosphate product.
[0059] Table 5
[0060] Al% Ca% Co% Cr% Cu% K% Mg% Na% 0.0135 0.0047 0.0003 0.00231 Not detected 0.0022 Not detected 0.0048 P% Ni% Fe% Mn% Ti% Zn% Pb% Fe:P ratio 17.28 0.0005 29.75 0.0049 0.0213 0.0014 Not detected 0.953
[0061] Comparative Example 3:
[0062] 1g of high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution was added to 28g of dilute phosphoric acid solution with a concentration of 40wt%, mixed and stirred, and then deionized water was added to the mixed solution to 200mL, and then the mixture was heated to 105℃ in an oil bath pot, the reaction time was 2h, and the solution pH was controlled at 1.10-1.20. After the reaction, the solution was filtered, 4g of reduced iron powder was added to the resulting solution, and then 0.6g of 30% H 2 O 2 , continue to stir and filter the solution, and then adjust the pH value to 2.0 with 10wt% ammonia solution. At this time, a white precipitate appears in the solution, and the white precipitate is filtered, washed and dried to obtain battery-grade iron phosphate FePO 4 product.
[0063] Preparation of iron phosphate FePO 4 The ICP analysis of the product is shown in Table 6. As can be seen from Table 6, when the pH value of the solution is 2.0, although more white ferric phosphate products are obtained, the iron precipitation rate in the solution is low and the iron-phosphorus ratio is somewhat low.
[0064] Table 6
[0065] Al% Ca% Co% Cr% Cu% K% Mg% Na% 0.0118 0.0043 0.0004 0.00227 Not detected 0.0023 Not detected 0.0045 P% Ni% Fe% Mn% Ti% Zn% Pb% Fe:P ratio 17.38 0.0007 28.34 0.0042 0.0201 0.0011 Not detected 0.903
[0066] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials, characterized in that: The following steps are involved: (1) adding powder of high-pressure hydrolysis product of cobalt-iron alloy acid leaching solution into deionized water, mixing and stirring, then adding phosphoric acid solution, stirring evenly to obtain a yellow mixed solution, heating for reaction, filtering to obtain a clear solution, and controlling its pH value to be 1.10-1.20; (2) Add reduced iron powder to the obtained clear solution while stirring, then add H2O2, continue stirring, and then filter; (3) The pH value of the solution obtained after filtering in step (2) is adjusted to between 2.85 and 3.50 to obtain a white precipitate, which is then filtered, washed, and dried to obtain a battery-grade iron phosphate FePO4 product.
2. The method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials according to claim 1, characterized in that: In step (1), the concentration of the phosphoric acid solution is 35-45wt%.
3. The method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials according to claim 1, characterized in that: In step (1), the heating reaction temperature is 100-110° C. and the time is 1-3 h.
4. The method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials according to claim 3, characterized in that: In step (1), the heating reaction temperature is 105° C. and the time is 2 h.
5. The method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials according to claim 1, characterized in that: In step (2), the amount of reduced iron powder added is such that the pH value of the solution after addition is between 1.50 and 1.
70.
6. The method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials according to claim 1, characterized in that: In step (2), the mass of H2O2 added is 50-70% of the mass of the powder of the high-pressure hydrolysis product of the cobalt-iron alloy acid leaching solution, and its concentration is 25-35wt%.
7. The method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials according to claim 1, characterized in that: In step (2), the stirring time is continued for 50-70 minutes, and the stirring temperature is room temperature.
8. The method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials according to claim 1, characterized in that: In step (3), the reagent used to adjust the pH value is ammonia water.
9. The method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials according to claim 8, characterized in that: In step (3), the concentration of the aqueous ammonia is 8-12 wt %.
10. The method for preparing battery-grade iron phosphate using high-pressure hydrolysis products of cobalt-iron alloy acid leaching solution as raw materials according to claim 9, characterized in that: In step (3), the concentration of the ammonia water is 10 wt %.
Citation Information
Patent Citations
Preparation of multi-position doped lithium iron phosphate positive electrode material and application thereof
CN101339994A
Magnetic sensor transformer for determining state of charge for iron phosphate lithium ion batteries
US20130149565A1