Preparation method of battery-grade iron phosphate with high iron-phosphorus ratio
Through segmented reaction control and mixed acid solution crystallization technology, the problem of insufficient iron-phosphorus ratio in lithium iron phosphate batteries has been solved, and the preparation of iron phosphate with high iron-phosphorus ratio and low impurities has been achieved, improving battery performance and production efficiency.
Patent Information
- Application Number
- CN202411063204.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to effectively increase the iron-phosphorus ratio of iron phosphate with existing technology, resulting in insufficient performance of lithium iron phosphate batteries and the inability to meet the market's stringent requirements for high iron-phosphorus ratios.
Through staged reaction control, the iron phosphate intermediate is generated at low temperature and within a specific pH value range, and a mixed acid solution is used for transcrystallization and aging. Combined with multi-step washing and calcination steps, the iron-phosphorus stoichiometric ratio is carefully controlled to maximize inhibition. The formation of iron hydroxide colloid increases the iron-phosphorus ratio of iron phosphate.
The iron-phosphorus ratio of ferric phosphate has been achieved to reach 0.980-0.998. The product has high tap density and excellent battery-level performance, significantly reducing impurity content and acid usage costs, and is suitable for large-scale industrial production.
Smart Images

Figure CN118723959A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium battery raw materials, and more specifically, to a method for preparing battery-grade iron phosphate with a high iron-to-phosphorus ratio. Background Art
[0002] Compared with traditional mechanical energy storage, electromagnetic energy storage and other energy storage methods, electrochemical energy storage has the advantages of high energy density, fast response speed, low maintenance cost, safety and convenience. It has become an important energy storage technology and has received extensive attention and research. Among them, lithium iron phosphate batteries have obvious advantages in the field of electrochemical energy storage due to their high energy density, excellent safety performance, long cycle life, and high cost performance. Especially in the field of power batteries, lithium iron phosphate batteries have occupied a dominant position in the market compared with other power batteries such as ternary batteries.
[0003] In current industrial production, the high-temperature solid-phase method uses iron phosphate, lithium carbonate, and an organic carbon source to fully mix and then calcine at high temperature in an inert protective gas to prepare lithium iron phosphate positive electrode materials. This process is widely regarded as the most mature and reliable method. A large number of studies have shown that the electrochemical properties of lithium iron phosphate materials are dominated by the physicochemical properties of iron phosphate. Among them, the iron-phosphorus ratio, a key indicator of iron phosphate quality, is one of the core factors that determine the performance of lithium iron phosphate materials, and the physicochemical properties of iron phosphate directly determine the comprehensive performance of lithium iron phosphate batteries. Therefore, it is of great significance to controllably limit the impurity content in iron phosphate and increase the iron-phosphorus ratio for the preparation of high-performance lithium iron phosphate positive electrode materials.
[0004] The iron-phosphorus ratio of iron phosphate obtained by existing preparation technology is usually around 0.970. As the market's requirements for the performance of lithium iron phosphate materials become higher and higher, battery manufacturers require the iron-phosphorus ratio of battery-grade iron phosphate to exceed 0.975, and some manufacturers expect it to reach 0.980. Although the market's requirements for the quality of iron phosphate are becoming increasingly stringent, there is still a lack of understanding and research on how to specifically improve the iron-phosphorus ratio.
[0005] A small number of patents have disclosed beneficial methods for improving the iron-phosphorus ratio of iron phosphate. Chinese patents CN109205584B and CN109368610B disclose adjustable iron-phosphorus ratios of iron phosphate to more than 0.98, and the core step is to add polyethylene glycol and phosphoric acid to a ferrous salt solution so that the subsequent reaction process solution is evenly distributed, reducing the presence of free iron ions, so that the prepared iron phosphate has a higher iron-phosphorus ratio. However, in some embodiments disclosed by Chinese patents CN116281917A and CN116332142A, an appropriate amount of polyethylene glycol or other surfactants are added to the iron phosphate preparation process, but the iron-phosphorus ratio does not reach 0.970. It is shown that during the preparation of iron phosphate, the addition of surfactants is conducive to the uniform distribution of chemical reactions in the solution, but may not necessarily be a determining factor in improving the iron-phosphorus ratio.
[0006] In addition, Chinese patents CN108455547B and CN112142025A disclose that in the process of preparing high iron-phosphorus ratio iron phosphate, the core step is to further add alkali solution at the end of the aging and crystallization process of the crude iron phosphate intermediate, and adjust the pH value of the aging reaction end point to 5.5-6.5, in order to eliminate the acid salts that may be produced by excessive phosphoric acid to increase the iron-phosphorus ratio. However, Chinese patent CN116281914A has a relatively detailed description of the aging and crystallization mechanism of the crude iron phosphate intermediate. The crude iron phosphate intermediate is easy to entrain more impurity ions in the form of chemical adsorption. The aging and crystallization process can strip the impurity ions from the iron phosphate into the aging solution. Therefore, at the end of the aging reaction of the crude iron phosphate intermediate, directly adding alkali solution to adjust the pH to 5.5-6.5 will cause the stripped impurity metal cations (except K+ and Na+ ions) to react and precipitate directly and quickly with the excess phosphate again, causing the impurity content of the final iron phosphate product to easily exceed the standard, and the product iron-phosphorus ratio is relatively low. Summary of the invention
[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for preparing battery-grade iron phosphate with a high iron-to-phosphorus ratio, which can stably prepare battery-grade iron phosphate with a high iron-to-phosphorus ratio and low impurities.
[0008] The above technical objectives of the present invention are achieved through the following technical solutions: a method for preparing battery-grade iron phosphate with a high iron-phosphorus ratio, comprising the following steps: S1. Under stirring conditions, add an iron source precursor and a surfactant to water, and then add a first acid solution to adjust the pH to 0.2-1 to obtain a first mixed solution; S2. Add a phosphorus source precursor to water under stirring conditions, and then add a second acid solution to adjust the pH to 0.5-0.9 to obtain a second mixed solution; S3. Under stirring conditions, adding the second mixed solution to the first mixed solution to obtain a third mixed solution, wherein the molar ratio of iron to phosphorus in the third mixed solution is 1:0.99-1.05; The temperature of the third mixed solution is maintained at 20-30° C., a pH adjuster is added to adjust the pH to 1-1.4, solid is precipitated, and the reaction is performed for 0.5-2 hours to obtain a slurry; The slurry is heated to 38-56° C., and then the pH adjuster is added to adjust the pH to 1.9-2.6, reacting for 1-5 hours, and solid-liquid separation to obtain an iron phosphate intermediate; S4, washing the ferric phosphate intermediate fully, adding it to a mixed acid solution, heating it to 85-98° C., aging it for 1-3 hours, and separating the solid from the liquid to obtain hydrated ferric phosphate; S5. The hydrated ferric phosphate is fully washed and dried, and calcined at 550-700° C. for 2-6 hours to obtain the target product.
[0009] In one embodiment, the iron source precursor includes at least one of ferric sulfate, ferric chloride, ferric nitrate and ferric acetate.
[0010] In one embodiment, the iron source precursor further includes at least one of ferrous sulfate and ferrous chloride; The S1 further comprises adding an oxidant to completely oxidize the ferrous ions of the iron source precursor into ferric ions.
[0011] In one embodiment, the surfactant includes one or more of polyethylene glycol, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer and polyvinyl pyrrolidone, and the mass ratio of the surfactant to the iron ions in the iron source precursor is 0.05-5:100.
[0012] In one embodiment, the phosphorus source precursor includes one or more of phosphoric acid, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, diammonium hydrogen phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, ammonium phosphate, sodium phosphate, potassium phosphate and phenylphosphonic acid.
[0013] In one embodiment, the first acid solution and the second acid solution include one or more of sulfuric acid, hydrochloric acid and nitric acid.
[0014] In one embodiment, the concentrations of iron salt and phosphate in the third mixed solution are both 0.1-2 mol / L.
[0015] In one embodiment, the pH regulator includes one of ammonia water, sodium hydroxide solution, potassium hydroxide solution, sodium bicarbonate solution, sodium carbonate solution, potassium bicarbonate solution, potassium carbonate solution, ammonium bicarbonate solution, ammonium carbonate solution and urea solution, and the concentration of the pH regulator is 3-25wt%.
[0016] In one embodiment, the mixed acid solution includes phosphoric acid and a third acid solution, wherein the molar ratio of phosphoric acid to the phosphoric acid precursor is 3-18:100, the molar ratio of phosphoric acid to the third acid solution is 100:0.03-40, and the third acid solution is nitric acid or hydrofluoric acid; The total concentration of the mixed acid solution is 0.8-4.6 wt %.
[0017] In one embodiment, in S4, the ferric phosphate intermediate is added to water at a temperature of 45-55° C., and the ferric phosphate intermediate is repeatedly pulped, washed and filtered until the pH of the washing liquid is ≥4.5, so as to fully wash the ferric phosphate intermediate; In S5, the hydrated ferric phosphate is added to water at a temperature of 45-55° C., and the hydrated ferric phosphate is repeatedly pulped, washed and filtered until the conductivity of the washing liquid is ≤150 μs / cm, so as to fully wash the hydrated ferric phosphate.
[0018] The above-mentioned method for preparing battery-grade iron phosphate with a high iron-phosphorus ratio has the following beneficial effects: First, the present invention controls the reaction by staged reaction. The ferric phosphate intermediate generated by the reaction at low temperature and pH value 1-1.4 has good dispersion and concentrated particle size distribution, and can be used as the embryo inducing reaction ions to further enrich, bond, stack and grow in the pH value range of 1.9-2.6, so that the prepared ferric phosphate particles are dense, and the final product has a high tap density of 0.8-1.3g / cm 3 ; Secondly, the present invention suppresses the formation of iron hydroxide colloid to the maximum extent through multiple steps. Even when the pH value of the solution is increased, the trace amount of iron hydroxide formed by local over-alkalinity can be fully dissolved and eliminated. At the same time, combined with the fine control of the iron-phosphorus stoichiometric ratio, the iron-phosphorus ratio of the product iron phosphate is 0.980-0.998. Thirdly, the mixed acid solution as a crystal-transforming agent in the aging and whitening step can significantly save the cost of acid use, and the aging and crystal-transforming time is shorter. In addition, the nitric acid / hydrofluoric acid and phosphoric acid in the mixed acid solution cooperate synergistically to fully dissociate the impurities entrained in the iron phosphate intermediate into the solution, so that the final iron phosphate quality can be significantly higher than the battery-grade requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The XRD diagram of the embodiment of the present invention and the corresponding standard PDF card; Figure 2 is a SEM image of iron phosphate in Example 1; Figure 3 is a SEM image of iron phosphate in Example 2; Figure 4 This is the SEM image of iron phosphate in Example 3. DETAILED DESCRIPTION
[0020] The present invention is described in further detail below in conjunction with the embodiments. It should be noted that the embodiments described below are intended to facilitate the understanding of the present invention and do not have any limiting effect on it. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs. When there is a conflict, the definitions in this specification shall prevail.
[0021] As used herein, the term "prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0022] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0023] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.
[0024] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0025] A method for preparing battery-grade iron phosphate with a high iron-phosphorus ratio comprises the following steps: S1. Under stirring conditions, add an iron source precursor and a surfactant to water, and then add a first acid solution to adjust the pH to 0.2-1 to obtain a first mixed solution; In step S1, a first acid solution is added to the iron source precursor solution to suppress the hydrolysis tendency of trivalent iron ions in the reaction iron source precursor during the preparation process.
[0026] S2. Add a phosphorus source precursor to water under stirring conditions, and then add a second acid solution to adjust the pH to 0.5-0.9 to obtain a second mixed solution; In step S2, after the phosphorus source precursor is fully dissolved, the pH value of the solution is greater than 2. After the pH value is adjusted with the second acid solution, the formation of trace amounts of iron hydroxide colloid caused by local over-alkalinity during the subsequent mixing of the iron source precursor solution and the phosphorus source precursor solution can be directly avoided.
[0027] Furthermore, in practical applications, the first acid solution and the second acid solution mostly use non-coordinating acids (except phosphoric acid).
[0028] S3. Under stirring conditions, the second mixed solution is added to the first mixed solution to obtain a third mixed solution, and the iron-phosphorus molar ratio in the third mixed solution is 1:0.99-1.05; the temperature of the third mixed solution is maintained at 20-30°C, a pH adjuster is added to adjust the pH of the third mixed solution to 1-1.4, a solid is precipitated, and the reaction is performed for 0.5-2h to obtain a slurry; the slurry is heated to 38-56°C, and a pH adjuster is added to adjust the pH of the slurry to 1.9-2.6, and the reaction is performed for 1-5h, and solid-liquid separation is performed to obtain an iron phosphate intermediate.
[0029] In step S3, the pH of the third mixed solution is adjusted by adding a pH regulator to obtain iron phosphate. In this process, there is a competitive relationship between the precipitation of iron phosphate and the precipitation of iron hydroxide. If the pH of the system is quickly adjusted to above 1.6, some iron ions will be precipitated in the form of iron hydroxide first, and the process of adding the pH regulator will cause local over-alkalinity, causing iron hydroxide to be entrained into the crude iron phosphate. This part of the iron hydroxide will increase the difficulty of subsequent crystallization because it is inside the iron phosphate intermediate. According to the K of iron hydroxide at room temperature sp =4×10 -38 , i.e. α(Fe 3+ )×[α(OH - )] 3 >K sp When the precipitation will precipitate, the water ion Kw is 10 -14 =C(OH - )×C(H + ), when Fe 3+ When the ion is 1 mol / L, pH>1.53·1 / 3log10[α(Fe 3+ )] -1 When Fe 3+ When the ion concentration is 0.1-2 mol / L, the corresponding pH of the iron hydroxide precipitation is 1.87-1.43. In practical applications, the third mixed solution begins to produce yellow-white iron phosphate precipitation when the pH value is adjusted to greater than 1. Adjusting the pH value of the third mixed solution to 1-1.4 can avoid the precipitation of iron hydroxide to the greatest extent and generate relatively pure crude iron phosphate particles.
[0030] Since local over-alkalinity is unavoidable during the use of pH regulators, the solution pH is adjusted to 1-1.4 and then maintained at low temperature (20-30°C) for 0.5-2h. This process can fully dissolve trace amounts of iron hydroxide formed by local over-alkalinity and further stabilize the crude iron phosphate particles initially formed.
[0031] Further raising the temperature (38-56°C) and adjusting the pH value of the slurry (1.9-2.6), the fine and well-dispersed crude ferric phosphate formed in the previous stage can serve as the embryo, which can promote the ferric ions and phosphate in the solution to be enriched, precipitated and layered on the surface of the embryo or in the gaps. Due to the sufficient formation of the crude ferric phosphate in the previous stage, the supersaturation of ferric ions has been greatly reduced. Raising the temperature and increasing the pH value of the slurry will not cause the trace free ferric ions to hydrolyze to form ferric hydroxide. When the concentration of ferric ions is 0.0001 mol / L, the pH of the ferric hydroxide precipitation is 2.86.
[0032] S4, fully washing the ferric phosphate intermediate, adding it to the mixed acid solution, heating it to 85-98°C, keeping it for aging for 1-3h, and separating the solid from the liquid to obtain hydrated ferric phosphate; The washed iron phosphate intermediate needs to be added to a mixed acid solution for aging and whitening. This process involves an orderly dissolution and recrystallization reaction process. If the acidity of the acidic solution is weak, the aging and whitening process will take a long time and the crystallization will be poor. If the acidity of the acidic solution is too strong, the iron phosphate intermediate will be partially dissolved in the acid solution and unable to crystallize.
[0033] S5. The hydrated ferric phosphate is fully washed and dried, and calcined at 550-700° C. for 2-6 hours to obtain the target product.
[0034] The present invention controls the reaction by staged reaction. The ferric phosphate intermediate generated by the reaction at low temperature and pH value range of 1-1.4 has good dispersion and concentrated particle size distribution, and can be used as the embryo inducing reaction ions to further enrich, bond, stack and grow in the pH value range of 1.9-2.6, so that the prepared ferric phosphate particles are dense, and the final product has a high tap density of 0.8-1.3g / cm 3 In addition, the formation of iron hydroxide colloid is suppressed to the maximum extent through multiple steps. Even when the pH value of the solution is increased, the trace amount of iron hydroxide formed by local over-alkalinity can be fully dissolved and eliminated. Combined with the fine control of the iron-phosphorus stoichiometric ratio, the iron-phosphorus ratio of the product iron phosphate is 0.980-0.998.
[0035] Specifically, the iron source precursor includes at least one of ferric sulfate, ferric chloride, ferric nitrate and ferric acetate.
[0036] Specifically, the iron source precursor further includes at least one of ferrous sulfate and ferrous chloride; S1 further includes adding an oxidant to completely oxidize the ferrous ions of the iron source precursor into trivalent ferrous ions.
[0037] In actual production, the iron source precursor can be selected from ferric salt or ferrous salt. When the iron source precursor is ferrous salt, S1 also includes adding an oxidant to completely oxidize the ferrous ions in the ferrous salt into trivalent ferrous ions; it should be further explained that the oxidant includes at least one of hydrogen peroxide, hypochlorite and ozone.
[0038] Specifically, the surfactant includes one or more of polyethylene glycol, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer and polyvinyl pyrrolidone, and the mass ratio of the surfactant to the iron ions in the iron source precursor is 0.05-5: 100. Adding the surfactant to the iron source precursor solution helps to evenly distribute the solution during the subsequent reaction and reduce the presence of free iron ions.
[0039] Specifically, the phosphorus source precursor includes one or more of phosphoric acid, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, diammonium hydrogen phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, ammonium phosphate, sodium phosphate, potassium phosphate and phenylphosphonic acid.
[0040] Specifically, the first acid solution and the second acid solution include one or more of sulfuric acid, hydrochloric acid and nitric acid. It should be further explained that when the iron source precursor is ferrous sulfate and the first acid solution and the second acid solution are sulfuric acid, the sulfur content in the finally obtained iron phosphate can be less than 25 mg / kg.
[0041] Specifically, the concentrations of iron salt and phosphate in the third mixed solution are both 0.1-2 mol / L.
[0042] Specifically, the pH adjuster includes one of ammonia water, sodium hydroxide solution, potassium hydroxide solution, sodium bicarbonate solution, sodium carbonate solution, potassium bicarbonate solution, potassium carbonate solution, ammonium bicarbonate solution, ammonium carbonate solution and urea solution, and the concentration of the pH adjuster is 3-25wt%.
[0043] Specifically, the mixed acid solution includes phosphoric acid and a third acid solution, wherein the molar ratio of phosphoric acid to the phosphoric acid precursor is 3-18:100, the molar ratio of phosphoric acid to the third acid solution is 100:0.03-40, and the third acid solution is nitric acid or hydrofluoric acid; the total concentration of the mixed acid solution is 0.8-4.6wt%.
[0044] In actual production, if a single phosphoric acid solution is used to age and whiten the ferric phosphate intermediate, in order to achieve the acidity required for dissolution and crystallization, the amount of phosphoric acid added will seriously exceed the stoichiometric ratio of iron and phosphorus, resulting in a relatively low iron and phosphorus content in the final ferric phosphate, and a long time is required for aging and whitening. The mixed solution of phosphoric acid and nitric acid / hydrofluoric acid is fully mixed with the ferric phosphate intermediate to react, and phosphoric acid can be used to multi-stage ionize H + ions combine with nitrate / fluoride ions to increase H + Ion utilization rate: dissolves trace amounts of impure phosphates or iron hydroxide complexes contained in the iron phosphate intermediates in a relatively short time, and dissolves the leached Fe 3+ The ions can fully react with the less excess phosphate to form hydrated iron phosphate with higher crystallinity.
[0045] The mixed acid solution can significantly save the cost of acid use as a crystal conversion agent in the aging and whitening step, and the aging and crystal conversion takes a short time. In addition, the nitric acid / hydrofluoric acid and phosphoric acid in the mixed acid solution work together to fully dissociate the impurities entrained in the iron phosphate intermediate into the solution, so that the final iron phosphate quality can be significantly higher than the battery grade requirements.
[0046] Specifically, in S4, the ferric phosphate intermediate is added to water at a temperature of 45-55°C, and the ferric phosphate intermediate is repeatedly pulped, washed and filtered until the pH of the washing liquid is ≥4.5, so as to fully wash the ferric phosphate intermediate; sufficient water washing of the ferric phosphate intermediate can significantly reduce the concentration of free impurity ions weakly adsorbed on the particle surface / pores.
[0047] In S5, the hydrated ferric phosphate is added to water at a temperature of 45-55° C., and the hydrated ferric phosphate is repeatedly pulped, washed and filtered until the conductivity of the washing liquid is ≤150 μs / cm, so as to fully wash the hydrated ferric phosphate. Example 1
[0048] S1, using pure water as the base liquid, adding ferric chloride and polyethylene glycol (molecular weight 8000) under stirring, the mass ratio of polyethylene glycol to ferric chloride is 0.99:100, and then adding 98wt% sulfuric acid to adjust the pH of the solution to 0.7 to obtain a first mixed solution with a concentration of 2mol / L; S2, using pure water as the base liquid, adding ammonium dihydrogen phosphate under stirring conditions, and then adding 98wt% sulfuric acid to adjust the solution pH to 0.8 to obtain a second mixed solution with a concentration of 2 mol / L; S3. Under stirring conditions, adding the second mixed solution to the first mixed solution, wherein the molar ratio of the added ferric chloride to diammonium phosphate is 1:1, to obtain a third mixed solution; The obtained third mixed solution was added into a reaction kettle, the temperature was maintained at 30° C., 25 wt % ammonia water was slowly added, the pH value of the third mixed solution was adjusted to 1.4, and after a yellow-white solid was precipitated, the mixture was reacted for 1 h to obtain a slurry; The slurry was further heated to 45° C., 25 wt % ammonia water was slowly added, the pH value of the slurry was adjusted to 2.4, the slurry was maintained for 3 hours, and then the slurry was solid-liquid separated to obtain a yellow-white iron phosphate intermediate; S4, adding the ferric phosphate intermediate to pure water at a temperature of 45° C., and repeatedly beating, washing, and filtering until the pH value of the washing liquid is not less than 4.5, to obtain the ferric phosphate intermediate after filtering; Further, a mixed acid solution composed of phosphoric acid and nitric acid is used as the base liquid, wherein the molar ratio of phosphoric acid to nitric acid in the mixed acid is 100:5, the molar ratio of phosphoric acid to ammonium dihydrogen phosphate in S3 is 10:100, and the total concentration of the mixed acid is 2.6wt%. The filtered iron phosphate intermediate is added to the mixed acid solution under stirring, and the temperature is raised to 90°C for aging for 2.5h, and then solid-liquid separation is performed to obtain a powdery white hydrated iron phosphate; S5. Add hydrated ferric phosphate to pure water at a temperature of 45°C, and repeat the pulping, washing and filter pressing processes until the conductivity of the washing liquid does not exceed 150μs / cm. The hydrated ferric phosphate after washing and filtration is fully dried at 70°C, and then calcined at 650°C for 3h to obtain battery-grade anhydrous ferric phosphate.
[0049] The XRD and SEM spectra of the anhydrous iron phosphate prepared in this example are as follows: Figure 1 , 2 shown. Example 2
[0050] S1, with pure water as the base liquid, ferrous sulfate was added under stirring, and hydrogen peroxide with a molar ratio of 1.8 times that of ferrous sulfate was added to fully oxidize ferrous ions to trivalent ferrous ions, polyethylene glycol (molecular weight 8000) was further added, the mass ratio of polyethylene glycol to ferrous sulfate was 0.24:100, and 98wt% sulfuric acid was added to adjust the pH of the solution to 0.8 to obtain a first mixed solution with a concentration of 1 mol / L; S2, using pure water as the base liquid, adding ammonium dihydrogen phosphate under stirring, and then adding 98wt% sulfuric acid to adjust the pH of the solution to 0.9 to obtain a second mixed solution with a concentration of 1 mol / L; S3. Under stirring conditions, adding the second mixed solution to the first mixed solution, wherein the molar ratio of the added ferrous sulfate to diammonium phosphate is 1:1.03, to obtain a third mixed solution; The third mixed solution was added to the reaction kettle, the temperature was maintained at 25° C., 20 wt % ammonium bicarbonate solution was slowly added, the pH value of the third mixed solution was adjusted to 1.3, and a yellow-white solid was precipitated, and the mixture was reacted for 1 h to obtain a slurry; The slurry was further heated to 50° C., 20 wt % ammonium bicarbonate solution was slowly added, the pH value of the slurry was adjusted to 2.3, the slurry temperature was maintained for 2 h, and then the slurry was solid-liquid separated to obtain a yellow-white iron phosphate intermediate; S4, adding the ferric phosphate intermediate to pure water at a temperature of 48° C., and repeatedly beating, washing, and filtering until the pH value of the washing liquid is not less than 4.5, to obtain the ferric phosphate intermediate after filtering; Further, a mixed acid solution of phosphoric acid and nitric acid is used as the base liquid, wherein the molar ratio of phosphoric acid to nitric acid in the mixed acid is 100:8, the molar ratio of phosphoric acid to ammonium dihydrogen phosphate in S3 is 8:100, and the total concentration of the mixed acid is 3.4wt%. The filtered iron phosphate intermediate is added to the mixed acid solution under stirring, and the temperature is raised to 94°C for aging for 2h, followed by solid-liquid separation to obtain a powdery white hydrated iron phosphate; S5. Add hydrated ferric phosphate to pure water at a temperature of 48°C, and repeat the pulping, washing, and filter pressing processes until the conductivity of the washing liquid does not exceed 150μs / cm. After sufficient washing and filtration, the hydrated ferric phosphate is fully dried at 90°C, and then calcined at 620°C for 4 hours to obtain battery-grade anhydrous ferric phosphate.
[0051] The XRD and SEM spectra of the anhydrous ferric phosphate prepared in this example are as follows: Figure 1 , 3 shown. Example 3
[0052] S1, using pure water as the base liquid, adding ferric sulfate and polyvinyl pyrrolidone (molecular weight 8000) under stirring, the mass ratio of polyvinyl pyrrolidone to ferric sulfate is 0.3:100, adding 98wt% sulfuric acid to adjust the solution pH to 0.6, and obtaining a first mixed solution with a concentration of 2.5mol / L; S2, using pure water as the base liquid, adding ammonium dihydrogen phosphate under stirring, and then adding 98wt% sulfuric acid to adjust the pH of the solution to 0.6 to obtain a second mixed solution with a concentration of 2.5mol / L; S3. Under stirring conditions, adding the second mixed solution to the first mixed solution, wherein the molar ratio of the added ferric sulfate to diammonium phosphate is 1:1, to obtain a third mixed solution; The third mixed solution was added to the reaction kettle, the temperature was maintained at 28° C., 25 wt % ammonium carbonate solution was slowly added, the pH value of the third mixed solution was adjusted to 1.3, and after a yellow-white solid was precipitated, the mixture was reacted for 1 h to obtain a slurry; The slurry was further heated to 52° C., 25 wt % ammonium carbonate solution was slowly added, the pH value of the slurry was adjusted to 2.1, the slurry temperature was maintained for 1 hour, and then the slurry was solid-liquid separated to obtain a yellow-white iron phosphate intermediate; S4, adding the ferric phosphate intermediate to pure water at a temperature of 49° C., and repeatedly beating, washing, and filtering until the pH value of the washing liquid is not less than 4.5, to obtain the ferric phosphate intermediate after filtering; Further, a mixed acid solution of phosphoric acid and hydrofluoric acid is used as the base liquid, wherein the molar ratio of phosphoric acid to hydrofluoric acid in the mixed acid is 100:4, the molar ratio of phosphoric acid to ammonium dihydrogen phosphate in S3 is 11:100, and the total concentration of the mixed acid is 2wt%. The fully filtered iron phosphate intermediate is added to the mixed acid solution under stirring, and the temperature is raised to 88°C for aging for 3h, and then solid-liquid separation is performed to obtain a pink-white hydrated iron phosphate; S5. Add hydrated ferric phosphate to pure water at a temperature of 49°C, and repeatedly pulp, wash, and filter press until the conductivity of the washing liquid does not exceed 150μs / cm. After sufficient washing and filtration, the hydrated ferric phosphate is fully dried at 85°C, and then calcined at 680°C for 2h to obtain battery-grade anhydrous ferric phosphate.
[0053] The XRD and SEM spectra of the anhydrous ferric phosphate prepared in this example are as follows: Figure 1 , 4 shown.
[0054] Comparative Example 1 S1. Using pure water as the base liquid, add ferric sulfate and polyethylene glycol (molecular weight 8000) under stirring, the mass ratio of polyethylene glycol to ferric sulfate is 0.12:100, and obtain a first mixed solution with a concentration of 2.5 mol / L; S2, using pure water as the base liquid, adding ammonium dihydrogen phosphate under stirring to obtain a second mixed solution with a concentration of 2.5 mol / L; S3. Under stirring conditions, adding the second mixed solution to the first mixed solution, wherein the molar ratio of the added ferrous sulfate to ammonium phosphate is 1:1, to obtain a third mixed solution; The third mixed solution was added to the reactor, the temperature was maintained at 30°C, and 25 wt% ammonium carbonate solution was slowly added to raise the pH value of the third mixed solution to 2.3; The slurry was further heated to 50°C and maintained at the slurry temperature for 1 hour, and then the slurry was subjected to solid-liquid separation to obtain a yellow-white iron phosphate intermediate; S4, using phosphoric acid solution as the base liquid, the molar ratio of phosphoric acid to ammonium dihydrogen phosphate in S3 is 11:100, the concentration of phosphoric acid is 2.6wt%, adding the iron phosphate intermediate to the phosphoric acid solution under stirring, heating to 90°C and aging for 3h, and then solid-liquid separation to obtain pink-white hydrated iron phosphate; S5. Add hydrated ferric phosphate into pure water at a temperature of 45°C, and repeat the pulping, washing and filter pressing processes until the conductivity of the washing liquid does not exceed 150μs / cm. After sufficient washing and filtration, the hydrated ferric phosphate is fully dried at 90°C, and then calcined at 600°C for 4h to obtain an anhydrous ferric phosphate comparison sample.
[0055] As shown in Table 1, the performance indicators of Examples 1-3 of the present invention, Comparative Example 1 and commercially available iron phosphate are shown. The reference standard is the limit value and implementation of type I iron phosphate in the chemical industry standard "Iron Phosphate for Batteries" (HG / T 4701-2021).
[0056] project unit HG / T 4701-2021 Example 1 Example 2 Example 3 Comparative Example 1 Commercially available iron % 35.7-36.7 36.54 36.52 36.59 35.97 36.26 phosphorus % 20-21.1 20.5 20.42 20.48 20.69 20.88 Iron-phosphorus ratio 0.96-1 0.988 0.992 0.991 0.964 0.965 calcium % ≤0.01 0.0004 ND 0.0001 0.001 0.0003 magnesium % ≤0.06 0.0009 0.0008 0.0009 0.0024 0.014 sodium % ≤0.02 0.0011 0.0010 0.0014 0.0021 0.0002 Potassium % ≤0.02 0.0004 0.0003 0.0003 0.0009 0.0027 copper % ≤0.003 0.0001 0.0001 0.0001 0.0001 0.0001 Zinc % ≤0.015 0.0001 0.0005 0.0004 0.0012 0.002 manganese % ≤0.1 0.0007 0.0007 0.0006 0.0007 0.0231 aluminum % ≤0.05 0.0022 0.0019 0.0015 0.0028 0.001 titanium % ≤0.18 0.0005 0.0004 0.0004 0.0013 0.0004 sulfur % ≤0.03 0.0011 0.0023 0.002 0.0188 0.0146 Magnetic foreign matter % <![CDATA[≤2.5×10 -4 ]]> <![CDATA[4.5×10 -6 ]]> <![CDATA[3.2×10 -6 ]]> <![CDATA[3.6×10 -6 ]]> <![CDATA[8.8×10 -5 ]]> <![CDATA[3.9×10 -6 ]]> Tap density <![CDATA[g / cm 3 ]]> ≥0.6 0.91 1.02 0.98 0.74 0.81 Particle size D50 μm 1-9 4.03 5.13 4.33 2.40 2.03 Moisture % ≤0.5 0.4 0.33 0.38 0.29 0.32 Specific surface area <![CDATA[m 2 / g]]> 3-16 6.40 3.69 6.01 8.19 8.66 Table 1 The main difference between Example 1 and Example 2 is that the iron source precursors used are ferric chloride and ferrous sulfate, respectively, and the pH regulators are ammonia water and ammonium bicarbonate, respectively. The main difference between Example 2 and Example 3 is that the surfactants and mixed acid components used are different. Combined with the XRD and SEM images of the embodiments and the index data of Table 1, the iron phosphates of the embodiments all have good crystallization performance. Due to the different iron source precursors and pH regulators, the microscopic morphology of the iron phosphate in Example 1 presents spindle-shaped primary particles, the radial length of the primary particles is close to 1 μm, the particles are large and the agglomeration is not obvious; the microscopic morphology of the iron phosphate in Example 2 and Example 3 is amorphous, and the formation of the primary particles is due to the repeated stacking and growth of the embryos, and the primary particles grow more densely. By accurately suppressing the formation of iron hydroxide and regulating the stoichiometric ratio of iron and phosphorus, it is achieved that Examples 1-3 have a higher iron-phosphorus ratio (0.988, 0.992, 0.991) than Comparative Example 1 and commercially available iron phosphate. In addition, the preparation process cleverly regulates the growth process of the iron phosphate intermediate and the crystallization aging process. During the growth of the iron phosphate intermediate, a high-purity iron phosphate microparticle embryo was formed in a lower pH range. The embryo was used to further induce the coordination ions to bond on the surface of the embryo and near the pores to make the particles stack and grow; during the crystal transformation and aging process, the acidic environment provided by the mixed acid can quickly realize the crystal transformation process of the iron phosphate intermediate with less phosphate input. Through the regulation of the two important steps, the final prepared iron phosphate has a larger tap density (0.91, 1.02, 0.98 g / cm 3 ). However, due to the lack of the above treatment, the comparative example 1 and the commercially available iron phosphate adsorbed and carried impurity phosphate during the synthesis of the iron phosphate, which ultimately resulted in a low iron-phosphorus ratio, and the final conversion of iron hydroxide into iron oxide would affect the tap density of the iron phosphate, which was also relatively small.
[0057] As can be seen from Table 1, the sulfur content of the iron phosphates of Examples 1-3 is almost one order of magnitude lower than that of Comparative Example 1 and commercially available iron phosphates, and the metal impurity content of the iron phosphates of Examples 1-3 is also relatively low, which is mainly attributed to the three advantages of the unique method of the present invention: First, the iron phosphate synthesis step accurately suppresses the formation of iron hydroxide colloid, so that the particles adsorb less impurity ions; second, in the process of generating the crude iron phosphate intermediate, segmented formation is adopted, and the microparticle embryos are used to induce the enrichment and bonding of coordinated ions, which are further stacked and grown on the surface of the embryos and near the pores. The good ion coordination environment is conducive to the orderly growth of the iron phosphate intermediates, thereby reducing the entrainment of impurity compounds; third, by fully washing the crude iron phosphate intermediates with water, the impurity ions physically adsorbed on the surface of the particles can be removed to the maximum extent, and the chemically adsorbed impurities can be quickly stripped into the mother liquor through the mixed acid environment of the crystal transformation and aging step.
[0058] In summary, the preparation method provided by the present invention can effectively prepare battery-grade iron phosphate with a high iron-phosphorus ratio, obtain iron phosphate with a high tap density, have obvious effects, and the reaction process is relatively easy to control, which is conducive to the flexible production of lithium-ion battery materials with excellent performance in large-scale industrial processes.
[0059] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing battery-grade iron phosphate with a high iron-to-phosphorus ratio, characterized in that: The following steps are involved: S1. Under stirring conditions, add an iron source precursor and a surfactant to water, and then add a first acid solution to adjust the pH to 0.2-1 to obtain a first mixed solution; S2. Add a phosphorus source precursor to water under stirring conditions, and then add a second acid solution to adjust the pH to 0.5-0.9 to obtain a second mixed solution; S3. Under stirring conditions, adding the second mixed solution to the first mixed solution to obtain a third mixed solution, wherein the molar ratio of iron to phosphorus in the third mixed solution is 1:0.99-1.05; The temperature of the third mixed solution is maintained at 20-30° C., a pH adjuster is added to adjust the pH to 1-1.4, solid is precipitated, and the reaction is performed for 0.5-2 hours to obtain a slurry; The slurry is heated to 38-56° C., and then the pH adjuster is added to adjust the pH to 1.9-2.6, reacting for 1-5 hours, and solid-liquid separation to obtain an iron phosphate intermediate; S4, washing the ferric phosphate intermediate fully, adding it to a mixed acid solution, heating it to 85-98° C., aging it for 1-3 hours, and separating the solid from the liquid to obtain hydrated ferric phosphate; S5. The hydrated ferric phosphate is fully washed and dried, and calcined at 550-700° C. for 2-6 hours to obtain the target product.
2. The method for preparing a battery-grade iron phosphate with a high iron-to-phosphorus ratio according to claim 1, characterized in that: The iron source precursor includes at least one of ferric sulfate, ferric chloride, ferric nitrate and ferric acetate.
3. The method for preparing a battery-grade iron phosphate with a high iron-to-phosphorus ratio according to claim 2, characterized in that: The iron source precursor further includes at least one of ferrous sulfate and ferrous chloride; The S1 further comprises adding an oxidant to completely oxidize the ferrous ions of the iron source precursor into ferric ions.
4. The method for preparing a battery-grade iron phosphate with a high iron-to-phosphorus ratio according to claim 1, characterized in that: The surfactant includes one or more of polyethylene glycol, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer and polyvinyl pyrrolidone, and the mass ratio of the surfactant to the iron ions in the iron source precursor is 0.05-5:
100.
5. The method for preparing a battery-grade iron phosphate with a high iron-to-phosphorus ratio according to claim 1, characterized in that: The phosphorus source precursor includes one or more of phosphoric acid, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, diammonium hydrogen phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, ammonium phosphate, sodium phosphate, potassium phosphate and phenylphosphonic acid.
6. The method for preparing a battery-grade iron phosphate with a high iron-to-phosphorus ratio according to claim 1, characterized in that: The first acid solution and the second acid solution include one or more of sulfuric acid, hydrochloric acid, and nitric acid.
7. The method for preparing a battery-grade iron phosphate with a high iron-to-phosphorus ratio according to claim 1, characterized in that: The concentrations of the iron salt and the phosphate in the third mixed solution are both 0.1-2 mol / L.
8. The method for preparing a battery-grade iron phosphate with a high iron-to-phosphorus ratio according to claim 1, characterized in that: The pH regulator includes one of ammonia water, sodium hydroxide solution, potassium hydroxide solution, sodium bicarbonate solution, sodium carbonate solution, potassium bicarbonate solution, potassium carbonate solution, ammonium bicarbonate solution, ammonium carbonate solution and urea solution, and the concentration of the pH regulator is 3-25wt%.
9. The method for preparing battery-grade iron phosphate with a high iron-to-phosphorus ratio according to claim 1, characterized in that: The mixed acid solution comprises phosphoric acid and a third acid solution, wherein the molar ratio of phosphoric acid to the phosphoric acid precursor is 3-18:100, the molar ratio of phosphoric acid to the third acid solution is 100:0.03-40, and the third acid solution is nitric acid or hydrofluoric acid; The total concentration of the mixed acid solution is 0.8-4.6 wt %.
10. The method for preparing battery-grade iron phosphate with a high iron-to-phosphorus ratio according to claim 1, characterized in that: In S4, the ferric phosphate intermediate is added to water at a temperature of 45-55° C., and the ferric phosphate intermediate is repeatedly pulped, washed and filtered until the pH of the washing liquid is ≥4.5, so as to fully wash the ferric phosphate intermediate; In S5, the hydrated ferric phosphate is added to water at a temperature of 45-55° C., and the hydrated ferric phosphate is repeatedly pulped, washed and filtered until the conductivity of the washing liquid is ≤150 μs / cm, so as to fully wash the hydrated ferric phosphate.
Citation Information
Patent Citations
Preparation method of iron phosphate with high tap density, low sulfur and high iron-phosphorus ratio
CN115124012A
Cited By
Synthesis method of battery-grade iron phosphate
CN120793868A