Modified lignin derived hard carbon negative electrode material and preparation and application thereof

By modifying the preparation method of lignin-derived hard carbon, the stacking of aromatic rings is broken and a closed-pore structure is formed, which solves the problem of insufficient sodium storage capacity and rate performance of lignin-derived hard carbon and improves the electrochemical performance and resources of sodium-ion batteries. Utilization efficiency.

CN118723970AActive Publication Date: 2024-10-01GUANGDONG UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410721272.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01
Estimated Expiration
2044-06-05

AI Technical Summary

Technical Problem

In the existing technology, it is difficult for lignin-derived hard carbon to generate a closed-pore structure during the pyrolysis process, resulting in low sodium storage capacity and poor rate performance, making it difficult to meet the needs of negative electrode materials for sodium-ion batteries.

Method used

Ammonia-oxidized lignin or quaternized lignin is used as the carbon source, combined with cetyltrimethylammonium bromide and sodium dodecylbenzene sulfonate as dispersants and sodium carboxymethylcellulose and sodium alginate as The binder prepares modified lignin-derived hard carbon through steps such as carbonization, pickling, water washing, drying and high-temperature carbonization to break the π-π stacking of aromatic rings and form rich disordered short-range graphite domains and closed-pore structures.

Benefits of technology

The specific capacity and platform capacity of the hard carbon anode are increased, the electrochemical performance of the sodium-ion battery is enhanced, and the comprehensive utilization of resources and cost reduction are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723970A_ABST
    Figure CN118723970A_ABST
Patent Text Reader

Abstract

The invention discloses a modified lignin derived hard carbon negative electrode material as well as preparation and application thereof. According to the lignin-derived hard carbon material, ammoxidation or quaternization lignin is adopted as a lignin carbon source, the lignin carbon source is mixed with a dispersing agent and a binding agent in an aqueous solution, drying is performed, and staged carbonization is performed at high temperature in an inert gas atmosphere to obtain the hard carbon material. The prepared hard carbon negative electrode material has a relatively small specific surface area and a proper interlayer spacing, and has relatively high specific capacity, relatively good rate capability and cycling stability when being used as a sodium-ion battery negative electrode. The hard carbon preparation method has the characteristics of simplicity in operation, low cost and the like. The comprehensive utilization of industrial lignin resources is realized, and industrial popularization is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of comprehensive resource utilization and sodium ion batteries, and specifically relates to a modified lignin-derived hard carbon negative electrode material and a preparation method and application thereof. Background Art

[0002] The scarcity and high cost of lithium resources severely limit the widespread application of lithium-ion batteries in grid-scale energy storage. Due to the abundant reserves of sodium and the similar physical and chemical properties to lithium, sodium-ion batteries are considered to be one of the candidates for large-scale stationary energy storage. Designing and manufacturing reliable high-capacity anode materials is a challenge for the commercialization of sodium-ion batteries. The large size of sodium ions compared to lithium ions This makes it difficult to intercalate in graphite with a small interlayer spacing. Hard carbon anodes are the best choice for sodium battery anodes due to their large interlayer spacing (0.37-4.0nm) and abundant defect sites. Hard carbon anodes are mainly prepared by carbonization of precursors such as biomass, resins, and polymers. They have many advantages such as wide sources, low cost, and no pollution. They are the most studied anode materials, but their low sodium storage capacity and poor rate performance still limit the development of hard carbon anodes.

[0003] As an economical and sustainable carbon source, biomass has become one of the most commonly used precursors for preparing hard carbon anode materials for sodium-ion batteries. Lignin is the second largest biomass component in the plant kingdom after cellulose, and is mainly derived from the pulp and paper making process and the alcohol production process of the cellulose industry. As an oxygen-rich natural aromatic polymer, lignin's amorphous disordered structure is a prerequisite for the formation of hard carbon. Therefore, lignin is a promising hard carbon precursor for large-scale production.

[0004] Due to its rich aromatic ring structure, lignin is affected by π-π stacking during the carbonization process, which will cause a large number of graphite-like domains to exist in lignin-derived hard carbon. The large number of long-range ordered graphite domains in the graphite-like domains not only makes it difficult to form a closed-pore structure, but also limits the diffusion of sodium ions, making the sodium storage capacity of lignin-derived hard carbon relatively low and the rate performance relatively poor.

[0005] Patent application CN116514105A discloses a method for preparing hard carbon for negative electrode of sodium ion battery. The method increases the sodium storage capacity by doping lignin with phosphorus atoms to increase the adsorption sites of lignin-derived hard carbon. However, the improvement effect is not significant, and the reversible sodium storage capacity is only 278 mAh g -1. The reason is that the capacity provided by defect adsorption accounts for a low proportion of the total capacity. Therefore, it is difficult to increase the sodium storage capacity by increasing the adsorption sites. Among the sodium storage capacity contributions of hard carbon, the platform capacity accounts for the largest proportion, and the platform capacity mainly comes from the filling of metalloid sodium in the closed pores (Chemistry of Materials 2022, 34, 3489-3500). The regulation of the closed pore volume of lignin-derived hard carbon can achieve the regulation of sodium storage capacity. Chinese patent CN110921647B discloses a method for preparing a hard carbon negative electrode for a sodium ion battery. This patent regulates the pores of hard carbon derived from sodium lignin sulfonate through a self-template, but the excessively large openings make it difficult for the hard carbon to close at high temperatures to form a closed pore structure, resulting in the reversible sodium storage capacity of the hard carbon obtained by this method not being significantly improved, and its capacity is only 303mAh·g -1 .

[0006] The main reason that hinders lignin from generating closed-pore structures during pyrolysis is that the large amount of aromatic ring structures in lignin make it difficult to generate disordered short-range graphite domains due to the influence of π-π stacking during pyrolysis, and too many long-range graphite domains make it difficult for lignin-derived hard carbon to generate closed pores. Therefore, how to generate a large number of closed-pore structures in lignin-derived hard carbon during pyrolysis is a technical problem that needs to be solved at present. Summary of the invention

[0007] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing a modified lignin-derived hard carbon negative electrode material.

[0008] Another object of the present invention is to provide a modified lignin-derived hard carbon negative electrode material prepared by the above preparation method.

[0009] Another object of the present invention is to provide an application of the above-mentioned modified lignin-derived hard carbon negative electrode material.

[0010] Lignin-derived hard carbon with both large interlayer spacing and high closed-cell pore volume is conducive to providing more sodium storage active sites, thereby improving the specific capacity and platform capacity of the hard carbon negative electrode. The present invention uses ammonia oxidized lignin or quaternized lignin as a lignin carbon source, at least one of hexadecyltrimethylammonium bromide and sodium dodecylbenzenesulfonate as a dispersant, and at least one of sodium carboxymethyl cellulose and sodium alginate as a binder, and prepares lignin-derived hard carbon by carbonization, pickling, washing, filtration, drying, and carbonization. During the carbonization process, the modified ammonia oxidized lignin and quaternized lignin can effectively break the π-π stacking of aromatic rings during the pyrolysis process due to the presence of nitrogen-containing functional groups with low bond energy, thereby increasing the proportion of disordered short-range graphite domains, and the disordered stacking of short-range graphite domains will produce a rich closed-cell structure. The lignin-derived hard carbon material of the present invention can be used in electrochemical energy storage fields such as sodium ion battery negative electrodes.

[0011] The purpose of the present invention is achieved through the following technical solutions:

[0012] A method for preparing a modified lignin-derived hard carbon negative electrode material for a sodium ion battery comprises the following steps:

[0013] (1) uniformly mixing ammonia-oxidized lignin and / or quaternized lignin, a dispersant and a binder to obtain a precursor;

[0014] (2) The precursor is carbonized for the first time in a protective gas atmosphere, then pickled, washed with water, and dried, and then carbonized for the second time in a protective gas atmosphere to obtain a modified lignin-derived hard carbon negative electrode material for a sodium ion battery.

[0015] Preferably, the ammonia oxidized lignin in step (1) is prepared by the following method: using water as the reaction medium, subjecting ammonia water, lignin and hydrogen peroxide to a hydrothermal reaction in a hydrothermal kettle, removing water, and obtaining the ammonia oxidized lignin.

[0016] More preferably, the ammonia water is added in the form of an aqueous ammonia solution, the concentration of the aqueous ammonia solution is 10-30wt.%; the mass ratio of the aqueous ammonia solution to the lignin is (1-3):(2-5), more preferably (2.5-2.8):(2-5).

[0017] The hydrogen peroxide is added in the form of a hydrogen peroxide solution, the concentration of the hydrogen peroxide solution is 8-50 wt.%; the mass ratio of the hydrogen peroxide solution to the lignin is 1:(2-5), more preferably 1:2.

[0018] More preferably, the ammonia water is added in the form of an aqueous ammonia solution, the concentration of the aqueous ammonia solution is 10 to 30 wt.%, and the mass ratio of the aqueous ammonia solution to water is 1:10 to 20.

[0019] More preferably, the temperature of the hydrothermal reaction is 110-130° C., more preferably 130° C., and the time is 1-2 h, more preferably 1 h.

[0020] More preferably, the order of adding the ammonia water, lignin and hydrogen peroxide is: first add the ammonia water solution into the water, then add the lignin and stir and mix evenly, then add the hydrogen peroxide solution and continue to stir and mix evenly.

[0021] More preferably, the stirring and mixing time is 0.5 to 1 h.

[0022] More preferably, the lignin is at least one of enzymatic lignin extracted from biorefining residues, organic solvent lignin obtained from solvent pulping, and alkali lignin extracted from black liquor from alkali pulping.

[0023] Preferably, the quaternized lignin in step (2) is prepared by the following method: lignin and 3-chloro-2-hydroxypropyltrimethylammonium chloride are heated and reacted in an aqueous solution with a pH of 11 to 13, followed by dialysis and drying to obtain quaternized lignin.

[0024] More preferably, the lignin is at least one of enzymatic lignin extracted from biorefining residues, organic solvent lignin obtained from solvent pulping, and alkali lignin extracted from black liquor from alkali pulping.

[0025] More preferably, the mass ratio of the lignin to 3-chloro-2-hydroxypropyltrimethylammonium chloride is (1-2):1; more preferably 1:1.

[0026] More preferably, the heating reaction temperature is 80-90°C, more preferably 80°C; the time is 3-6h, more preferably 6h.

[0027] More preferably, the order of adding the lignin and 3-chloro-2-hydroxypropyltrimethylammonium chloride is: first add the lignin to water, adjust the pH to 11-13, and then add 3-chloro-2-hydroxypropyltrimethylammonium chloride; wherein the mass ratio of lignin to water is 1:(2-4), more preferably 1:4; the regulator for adjusting the pH is 10-20wt.% sodium hydroxide solution, more preferably 20wt.% sodium hydroxide solution.

[0028] More preferably, the drying temperature is 65-80° C. and the drying time is 8-12 hours.

[0029] Preferably, in step (1), the mass ratio of lignin, dispersant and binder is 10:(0.5-1):(0.5-1), more preferably 10:0.5:0.5, wherein lignin refers to ammonia-oxidized lignin and / or quaternized lignin.

[0030] Preferably, the dispersant in step (1) is at least one of hexadecyltrimethylammonium bromide and sodium dodecylbenzenesulfonate.

[0031] Preferably, the binder in step (1) is at least one of sodium carboxymethyl cellulose and sodium alginate.

[0032] Preferably, the method for uniform mixing in step (1) is: adding ammonia oxidized lignin and / or quaternized lignin and a dispersant to water and stirring evenly, then adding a binder and continuing to stir evenly, and drying to obtain a precursor.

[0033] More preferably, the drying temperature is 60 to 80° C. and the drying time is 12 to 24 hours.

[0034] More preferably, the ratio of lignin to water is (10-20) g: (100-500) mL, more preferably 20 g: (100-250) mL, wherein lignin refers to ammonia-oxidized lignin and / or quaternized lignin.

[0035] More preferably, the stirring time is 2 to 5 hours.

[0036] Preferably, the protective gas in step (2) is at least one of nitrogen, argon and helium.

[0037] Preferably, the temperature of the first carbonization in step (2) is 400-800°C, more preferably 600-700°C, and the time is 0.5-5h, more preferably 2h; the temperature of the second carbonization is 1000-1500°C, more preferably 1200-1500°C, and the time is 2-6h, more preferably 2-5h.

[0038] Preferably, the heating rates of the two carbonizations in step (2) are both 1-10°C / min, more preferably 5°C / min, and the flow rate of the protective gas is 2-100 mL / min, more preferably 60 mL / min.

[0039] Preferably, the acid used for pickling in step (2) is at least one of 0.5-2 mol / L dilute hydrochloric acid, 0.5-2 mol / L sulfuric acid and 0.5-2 mol / L nitric acid, and pickling refers to immersing the carbonized material in the acid and stirring for 2-48 hours.

[0040] Preferably, the water washing in step (2) refers to immersing the carbonized material in water and stirring for 12 to 48 hours, and then filtering. The acid washing is followed by water washing and then drying; the drying temperature is 60 to 80° C. and the drying time is 8 to 12 hours.

[0041] The above preparation method obtains a modified lignin-derived hard carbon negative electrode material for sodium ion batteries.

[0042] The specific surface area of ​​the modified lignin-derived hard carbon negative electrode material for sodium ion batteries is 5 to 30 m 2 / g, with the characteristics of few open pores and many closed pores; the sodium metal half-cell assembled in 1mol / L NaPF6 in DME electrolyte was tested at different current densities, and its specific capacity was 300~360mAh·g -1 .

[0043] The above-mentioned modified lignin-derived hard carbon negative electrode material for sodium ion batteries is used in sodium ion batteries.

[0044] The present invention aims to utilize cheap lignin for modification to prepare a hard carbon negative electrode for sodium ion batteries. Traditional preparation methods usually use alkali metal salts as templates to form pores. The mass ratio of the template to carbon is high, which causes the hard carbon to have too many open pores, a large specific surface area, and poor sodium storage performance. The present invention modifies lignin, adds a dispersant and mixes it evenly with the lignin carbon source, and adds a binder to make the lignin carbon source structure dense, thereby reducing the preparation cost and realizing the comprehensive utilization of resources. The hard carbon negative electrode material obtained after carbonization has a small specific surface area and a large number of closed-pore structures, and also has good electrochemical properties.

[0045] In addition, the preparation method of the modified lignin-derived hard carbon negative electrode material for sodium ion batteries proposed in the present invention has the advantages of no corrosion to equipment, simple preparation process, and low preparation cost, which is conducive to large-scale production.

[0046] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0047] (1) The present invention uses lignin, which is abundant in source and low in cost, as a matrix, performs ammonia oxidation or quaternization modification on lignin, changes the pyrolysis behavior of lignin, disperses the lignin carbon source through a dispersant, and then uses a binder to make the lignin carbon source structure dense, and finally obtains lignin-derived hard carbon for sodium ion batteries through low-temperature carbonization, acid washing and high-temperature carbonization. Therefore, the present invention has the advantages of being environmentally friendly, simple in preparation process and low in cost.

[0048] (2) The carbon material obtained in the present invention has a small specific surface area and a rich closed-pore structure. The rich closed-pore structure can provide pore-filled sodium storage micro-points for the platform capacity, thereby improving the capacity and rate performance of the sodium ion battery.

[0049] (3) The present invention uses cheap lignin resources to prepare hard carbon materials that can be used for the negative electrode of sodium ion batteries, thereby achieving comprehensive utilization of resources in the material preparation process, which is conducive to industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 Flow chart of the preparation of lignin-derived hard carbon for sodium-ion batteries in this application.

[0051] Figure 2 This is the XRD pattern of the quaternary ammonium lignin derived hard carbon (QALHC) in Example 1.

[0052] Figure 3 This is the Raman graph of the quaternary ammonium lignin derived hard carbon (QALHC) in Example 1.

[0053] Figure 4 This is the SAXS pattern of the quaternary ammonium lignin derived hard carbon (QALHC) in Example 1.

[0054] Figure 5 This is the SEM image of the quaternary ammonium lignin derived hard carbon (QALHC) of Example 1 (magnification is 10000 times).

[0055] Figure 6 This is the nitrogen adsorption-desorption isotherm of the quaternary ammonium lignin derived hard carbon (QALHC) in Example 1.

[0056] Figure 7 This is the pore size distribution diagram of the quaternary ammonium lignin derived hard carbon (QALHC) in Example 1.

[0057] Figure 8 This is a dotted line graph showing the variation of specific capacity with current density of quaternized lignin-derived hard carbon (QALHC) used as the negative electrode of sodium ion battery in Example 1.

[0058] Fig. 9 Example 1: Quaternary ammonium lignin derived hard carbon (QALHC) used as a negative electrode for sodium ion batteries at 1 A·g -1 Cycling performance at current density.

[0059] Fig.10 This is the SAXS graph of the lignin-derived hard carbon (QALHC) of Comparative Example 1. DETAILED DESCRIPTION

[0060] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0061] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All raw materials, reagents, etc., whose manufacturers are not specified, are conventional products that can be purchased commercially.

[0062] Example 1

[0063] (1) Dissolve 50 g of dry enzymatic lignin in 200 mL of deionized water, adjust the pH to 12.0 with 20 wt.% NaOH, add 50 g of 3-chloro-2-hydroxypropyltrimethylammonium chloride, and react at 80°C for 6 h; use a dialysis bag (1000 Da MWCO) to remove unreacted small molecules and inorganic salts, dialyze and purify the solution, dry and grind to obtain quaternized lignin (QAL).

[0064] (2) 20 g of quaternized lignin, 1 g of hexadecyltrimethylammonium bromide and 250 mL of ultrapure water were added into a 500 mL beaker in sequence, stirred to fully mix the quaternized lignin and hexadecyltrimethylammonium bromide, and then continued to stir for 3 h.

[0065] (3) Add 1 g of sodium carboxymethyl cellulose to the solution of step (2) and stir for 3 h.

[0066] (4) The solution of step (3) is placed in an oven at 75° C. to dry the solution to obtain a solid.

[0067] (5) The solid from step (4) was heated to 700°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min and carbonized for 2 h. After the reaction, it was soaked in 1 mol / L hydrochloric acid for 12 h, washed with deionized water for 12 h, vacuum filtered and dried at 75°C for 10 h to obtain a quaternary ammonium lignin-derived porous carbon, named QAL-700.

[0068] (6) QAL-700 was heated to 1400 °C at a heating rate of 5 °C / min and carbonized for 2 h under a nitrogen atmosphere with a gas flow rate of 60 mL / min to obtain quaternary ammonium lignin-derived hard carbon, named QALHC.

[0069] The prepared QALHC has a 7.1m 2 / g small specific surface area. The X-ray diffraction (XRD) and Raman (Raman) patterns of QALHC hard carbon negative electrode are shown in Figure 2 and Figure 3 As shown, Figure 2 Two broad peaks appear near 23° and 44°, corresponding to the (002) and (100) crystal planes of the carbon material. The interlayer spacing of QALHC is calculated to be 0.380nm, and the ID1 / IG value is calculated to be 2.40 after fitting. This shows that QALHC has a disordered carbon layer structure and a large interlayer spacing, which is conducive to the intercalation of sodium ions.

[0070] QALHC, conductive carbon black and PVDF (polyvinylidene fluoride) were mixed in a mass ratio of 8:1:1 and coated on a copper foil, which was then dried and cut into circular electrode sheets with a radius of 6 mm for later use.

[0071] Scanning electron microscope (SEM) images of QALHC are shown below: Figure 5 As shown in the figure, the morphology of the hard carbon derived from quaternary ammonium lignin is blocky, with a relatively smooth surface and some micropores.

[0072] Figure 6 and Figure 7 Nitrogen adsorption-desorption curve and pore size distribution diagram of QALHC. Figure 6 The increase in nitrogen adsorption in the low adsorption pressure region indicates the presence of micropores, while an obvious increase in nitrogen adsorption and a hysteresis adsorption ring appear at high adsorption pressure, indicating the presence of mesopores. Figure 7 The pore size distribution diagram also verifies this conclusion.

[0073] The prepared sodium ion battery electrode sheet was used as the negative electrode, the sodium metal sheet as the positive electrode, and 1 mol / LNaPF6 inDME as the electrolyte to assemble a sodium ion button battery, and the electrochemical performance of QALHC was tested.

[0074] Figure 8 The dotted line graph of the specific capacity of QALHC as the negative electrode of sodium ion battery changes with the current density. -1 At a current density of 354 mAh g -1 The specific capacity at 5A·g -1 Still has 134mAh g -1 The specific capacity of QALHC indicates that it has excellent rate performance when applied to the negative electrode of sodium-ion batteries. Fig. 9 This shows that the half-cell is -1 The capacity retention rate is 87.1% after 1000 cycles.

[0075] Example 2

[0076] (1) Add 10 g of commercially available ammonia solution (25-28 wt.%) to 200 mL of deionized water; slowly add 10 g of dry enzymatic lignin and stir for 30 minutes; add 5 g of a quantitative commercially available hydrogen peroxide solution (30 wt.%), continue stirring for 30 minutes, and then transfer to a hydrothermal reactor; perform hydrothermal reaction at 130° C. for 1 hour; after the hydrothermal reactor is cooled, the reaction solution is rotary evaporated to remove water and unreacted products, and then vacuum dried at 80° C. and ground to obtain ammonia oxidized lignin (AOL).

[0077] (2) 20 g of ammonia-oxidized lignin, 1 g of hexadecyltrimethylammonium bromide, and 100 mL of ultrapure water were added into a 500 mL beaker in sequence, and the mixture was stirred to fully mix the ammonia-oxidized lignin and hexadecyltrimethylammonium bromide, and then continued to stir for 3 h.

[0078] (3) Add 1 g of sodium carboxymethyl cellulose to the solution of step (2) and stir for 3 h.

[0079] (4) The solution of step (3) is placed in an oven at 75° C. to dry the solution to obtain a solid.

[0080] (5) The solid from step (4) was heated to 700°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min and carbonized for 2 h. After the reaction, it was soaked in 1 mol / L hydrochloric acid for 12 h, washed with deionized water for 12 h, vacuum filtered and dried at 75°C for 10 h to obtain ammonia-oxidized lignin-derived porous carbon, named AOL-700.

[0081] (6) AOL-700 was heated to 1500 °C at a heating rate of 5 °C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min and carbonized for 4 h to obtain ammonia-oxidized lignin-derived hard carbon, named AOLHC.

[0082] (6) The prepared AOLHC has a 20.3m 2 / g smaller specific surface area.

[0083] AOLHC, conductive carbon black and PVDF (polyvinylidene fluoride) were mixed in a mass ratio of 8:1:1 and coated on a copper foil, which was dried and cut into circular electrode sheets with a radius of 6 mm for later use.

[0084] The prepared sodium ion battery electrode sheet was used as the negative electrode, the sodium metal sheet as the positive electrode, and 1 mol / LNaPF6 inDME as the electrolyte to assemble a sodium ion button battery, and the electrochemical performance of AOLHC was tested.

[0085] AOLHC at 0.05A·g -1 At a current density of 339 mAh g -1 The specific capacity at 5A·g -1 Still has 131mAh·g -1 The specific capacity of AOLHC indicates that it has excellent rate performance when applied to the negative electrode of sodium ion batteries.

[0086] Example 3

[0087] (1) Dissolve 100 g of dry enzymatic lignin in 200 mL of deionized water, adjust the pH to 12.0 with 20 wt.% NaOH, add 50 g of 3-chloro-2-hydroxypropyltrimethylammonium chloride, and react at 90°C for 3 h; use a dialysis bag (1000 Da MWCO) to remove unreacted small molecules and inorganic salts, dialyze and purify the solution, dry and grind to obtain quaternized lignin (QAL).

[0088] (2) 20 g of quaternized lignin, 2 g of hexadecyltrimethylammonium bromide and 250 mL of ultrapure water were added into a 500 mL beaker in sequence, stirred to fully mix the quaternized lignin and hexadecyltrimethylammonium bromide, and then continued to stir for 3 h.

[0089] (3) Add 2 g of sodium carboxymethyl cellulose to the solution of step (2) and stir for 3 h.

[0090] (4) The solution of step (3) is placed in an oven at 75° C. to dry the solution to obtain a solid.

[0091] (5) The solid from step (4) was heated to 600°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min and carbonized for 2 h. After the reaction, it was soaked in 1 mol / L hydrochloric acid for 12 h, washed with deionized water for 12 h, vacuum filtered and dried at 75°C for 10 h to obtain a quaternary ammonium lignin-derived porous carbon named QAL-600.

[0092] (6) QAL-600 was heated to 1200 °C at a heating rate of 5 °C / min and carbonized for 6 h under a nitrogen atmosphere with a gas flow rate of 60 mL / min to obtain a quaternary ammonium lignin-derived hard carbon, named QALHC-2.

[0093] QALHC-2 at 0.05A·g -1 At a current density of 348 mAh g -1 The specific capacity at 5A·g -1 Still has 123mAh g -1 The specific capacity of QALHC-2 indicates that it has excellent rate performance when used as a negative electrode for sodium-ion batteries.

[0094] Example 4

[0095] (1) Add 20 g of commercially available ammonia solution (25-28 wt.%) to 200 mL of deionized water; slowly add 40 g of dry enzymatic lignin and stir for 30 minutes; add 8 g of a quantitative commercially available hydrogen peroxide solution (30 wt.%), continue stirring for 30 minutes, and then transfer to a hydrothermal reactor; perform hydrothermal reaction at 110° C. for 2 h; after the hydrothermal reactor is cooled, the reaction solution is rotary evaporated to remove water and unreacted products, and then vacuum dried at 80° C. and ground to obtain ammonia oxidized lignin (AOL).

[0096] (2) 20 g of ammonia-oxidized lignin, 2 g of hexadecyltrimethylammonium bromide, and 100 mL of ultrapure water were added to a 500 mL beaker in sequence, and the mixture was stirred to fully mix the ammonia-oxidized lignin and hexadecyltrimethylammonium bromide, and then continued to stir for 3 h.

[0097] (3) Add 2 g of sodium carboxymethyl cellulose to the solution of step (2) and stir for 3 h.

[0098] (4) The solution of step (3) is placed in an oven at 75° C. to dry the solution to obtain a solid.

[0099] (5) The solid from step (4) was heated to 600° C. at a heating rate of 5° C. / min in a nitrogen atmosphere with a gas flow rate of 60 mL / min and carbonized for 2 h. After the reaction, it was soaked in 1 mol / L hydrochloric acid for 12 h, washed with deionized water for 12 h, vacuum filtered and dried at 75° C. for 10 h to obtain ammonia-oxidized lignin-derived porous carbon, named AOL-600.

[0100] (6) AOL-600 was heated to 1300 °C at a heating rate of 5 °C / min and carbonized for 5 h under a nitrogen atmosphere with a gas flow rate of 60 mL / min to obtain ammonia-oxidized lignin-derived hard carbon, named AOLHC-2.

[0101] AOLHC-2 at 0.05A·g -1 At a current density of 344 mAh g -1 The specific capacity at 5A·g -1 Still has 118mAh g -1 The specific capacity of AOLHC indicates that it has excellent rate performance when applied to the negative electrode of sodium ion batteries.

[0102] Comparative Example 1

[0103] (1) 20 g of enzymatically hydrolyzed lignin, 1 g of hexadecyltrimethylammonium bromide, and 250 mL of ultrapure water were added to a 500 mL beaker in sequence, stirred to fully mix the lignin and hexadecyltrimethylammonium bromide, and then continued to stir for 3 h.

[0104] (2) Add 1 g of sodium carboxymethyl cellulose to the solution of step (1) and stir for 3 h.

[0105] (3) The solution of step (2) is placed in an oven at 75° C. to dry the solution to obtain a solid.

[0106] (4) The solid obtained in step (3) was heated to 700°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min and carbonized for 2 h. After the reaction, it was soaked in 1 mol / L hydrochloric acid for 12 h, washed with deionized water for 12 h, vacuum filtered and dried at 75°C for 10 h to obtain a lignin-derived porous carbon named AL-700.

[0107] (5) AL-700 was carbonized at 1400 °C at a heating rate of 5 °C / min for 2 h under a nitrogen atmosphere with a gas flow rate of 60 mL / min to obtain lignin-derived hard carbon, named ALHC.

[0108] The prepared ALHC has a 2.9m 2 / g of small specific surface area. ALHC, conductive carbon black and PVDF (polyvinylidene fluoride) were mixed in a mass ratio of 8:1:1 and coated on copper foil. After drying, they were cut into circular electrode sheets with a radius of 6 mm for standby use. The prepared sodium ion battery electrode sheet was used as the negative electrode, the sodium metal sheet as the positive electrode, and 1mol / LNaPF6 in DME as the electrolyte to assemble a sodium ion button cell, and the electrochemical performance of ALHC was tested.

[0109] At 0.05A·g -1 At a current density of 301 mAh g -1 The specific capacity at 5A·g -1 99mAh·g -1 The specific capacity of ALHC indicates that the rate performance of ALHC applied to the negative electrode of sodium ion battery is worse than that in Examples 1 and 2.

[0110] Comparative Example 2

[0111] (1) 20 g of ammonia-oxidized lignin (obtained in Example 2), 1 g of hexadecyltrimethylammonium bromide and 100 mL of ultrapure water were added to a 500 mL beaker in sequence, stirred to fully mix the ammonia-oxidized lignin and hexadecyltrimethylammonium bromide, and then continued to stir for 3 h.

[0112] (3) Add 1 g of sodium carboxymethyl cellulose to the solution of step (2) and stir for 3 h.

[0113] (4) The solution of step (3) is placed in an oven at 75° C. to dry the solution to obtain a solid.

[0114] (5) The solid from step (4) was heated to 700°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min and carbonized for 2 h. After the reaction, it was soaked in 1 mol / L hydrochloric acid for 12 h, washed with deionized water for 12 h, vacuum filtered and dried at 75°C for 10 h to obtain ammonia-oxidized lignin-derived porous carbon, named AOL-700.

[0115] (6) AOL-700 was heated to 900 °C at a heating rate of 5 °C / min and carbonized for 2 h under a nitrogen atmosphere with a gas flow rate of 60 mL / min to obtain ammonia-oxidized lignin-derived hard carbon, named AOLHC-3.

[0116] Comparative Example 3

[0117] (1) 20 g of quaternized lignin (obtained in Example 1), 1 g of hexadecyltrimethylammonium bromide and 250 mL of ultrapure water were added to a 500 mL beaker in sequence, stirred to fully mix the quaternized lignin and hexadecyltrimethylammonium bromide, and then continued to stir for 3 h.

[0118] (3) Add 1 g of sodium carboxymethyl cellulose to the solution of step (2) and stir for 3 h.

[0119] (4) The solution of step (3) is placed in an oven at 75° C. to dry the solution to obtain a solid.

[0120] (5) The solid from step (4) was heated to 700°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min and carbonized for 2 h. After the reaction, it was soaked in 1 mol / L hydrochloric acid for 12 h, washed with deionized water for 12 h, vacuum filtered and dried at 75°C for 10 h to obtain a quaternary ammonium lignin-derived porous carbon, named QAL-700.

[0121] (6) QAL-700 was heated to 1700 °C at a heating rate of 5 °C / min and carbonized for 2 h under a nitrogen atmosphere with a gas flow rate of 60 mL / min to obtain a quaternary ammonium lignin-derived hard carbon named QALHC-3.

[0122] Table 1 Capacity of negative electrode materials of Examples 1 to 4 and Comparative Examples 1 to 3

[0123]

[0124] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a modified lignin-derived hard carbon negative electrode material, characterized in that: The following steps are involved: (1) uniformly mixing ammonia-oxidized lignin and / or quaternized lignin, a dispersant and a binder to obtain a precursor; (2) The precursor is carbonized for the first time in a protective gas atmosphere, then pickled, washed with water, and dried, and then carbonized for the second time in a protective gas atmosphere to obtain a modified lignin-derived hard carbon negative electrode material.

2. The method for preparing a modified lignin-derived hard carbon negative electrode material according to claim 1, characterized in that: The ammonia-oxidized lignin in step (1) is prepared by the following method: using water as a reaction medium, subjecting ammonia water, lignin and hydrogen peroxide to a hydrothermal reaction in a hydrothermal kettle, removing water, and obtaining the ammonia-oxidized lignin; The ammonia water is added in the form of an ammonia solution, the concentration of the ammonia solution is 10-30 wt.%; the mass ratio of the ammonia solution to the lignin is (1-3): (2-5); The hydrogen peroxide is added in the form of a hydrogen peroxide solution, the concentration of the hydrogen peroxide solution is 8-50 wt.%; the mass ratio of the hydrogen peroxide solution to the lignin is 1:(2-5); The temperature of the hydrothermal reaction is 110-130°C and the time is 1-2h; The lignin is at least one of enzymatic lignin extracted from biorefining residues, organic solvent lignin obtained from solvent pulping, and alkali lignin extracted from black liquor from alkali pulping.

3. The method for preparing a modified lignin-derived hard carbon negative electrode material according to claim 1, characterized in that: The quaternized lignin in step (2) is prepared by the following method: heating lignin and 3-chloro-2-hydroxypropyltrimethylammonium chloride in an aqueous solution with a pH of 11 to 13 for reaction, followed by dialysis and drying to obtain quaternized lignin; The mass ratio of the lignin to 3-chloro-2-hydroxypropyltrimethylammonium chloride is (1-2):1; the heating reaction temperature is 80-90°C and the time is 3-6h; The lignin is at least one of enzymatic lignin extracted from biorefining residues, organic solvent lignin obtained from solvent pulping, and alkali lignin extracted from black liquor from alkali pulping.

4. The method for preparing a modified lignin-derived hard carbon negative electrode material according to claim 1, characterized in that: In step (1), the mass ratio of lignin, dispersant and binder is 10:(0.5-1):(0.5-1), wherein lignin refers to ammonia-oxidized lignin and / or quaternized lignin; The dispersant in step (1) is at least one of hexadecyltrimethylammonium bromide and sodium dodecylbenzenesulfonate; The binder in step (1) is at least one of sodium carboxymethyl cellulose and sodium alginate.

5. The method for preparing a modified lignin-derived hard carbon negative electrode material according to claim 1, characterized in that: The temperature of the first carbonization in step (2) is 400-800° C. and the time is 0.5-5 h; The temperature of the second carbonization is 1000-1500°C and the time is 2-6 hours.

6. The method for preparing a modified lignin-derived hard carbon negative electrode material according to claim 1, characterized in that: The method for uniform mixing in step (1) is as follows: adding ammonia oxidized lignin and / or quaternized lignin and a dispersant to water and stirring evenly, then adding a binder and continuing to stir evenly, and drying to obtain a precursor; the ratio of lignin to water is (10-20) g: (100-500) mL, wherein the lignin refers to ammonia oxidized lignin and / or quaternized lignin; The protective gas in step (2) is at least one of nitrogen, argon and helium; The heating rates of the two carbonizations in step (2) are both 1-10° C. / min, and the flow rate of the protective gas is 2-100 mL / min; The acid used for pickling in step (2) is at least one of 0.5-2 mol / L dilute hydrochloric acid, 0.5-2 mol / L sulfuric acid and 0.5-2 mol / L nitric acid. Pickling refers to immersing the carbonized material in the acid and stirring for 2-48 hours.

7. The method for preparing a modified lignin-derived hard carbon negative electrode material according to claim 2, characterized in that: The ammonia water is added in the form of an ammonia solution, the concentration of the ammonia solution is 10-30 wt.%; the ratio of the ammonia solution to water is 1: (5-20); The order of adding the ammonia water, lignin and hydrogen peroxide is: first add the ammonia solution into the water, then add the lignin and stir and mix evenly, then add the hydrogen peroxide solution and continue to stir and mix evenly.

8. The method for preparing a modified lignin-derived hard carbon negative electrode material according to claim 3, characterized in that: The order of adding the lignin and 3-chloro-2-hydroxypropyltrimethylammonium chloride is as follows: firstly adding the lignin into water, adjusting the pH value to 11-13, and then adding the 3-chloro-2-hydroxypropyltrimethylammonium chloride; wherein the mass ratio of the lignin to the water is 1:(2-4), and the regulator for adjusting the pH value is a 10-20wt.% sodium hydroxide solution.

9. A modified lignin-derived hard carbon negative electrode material obtained by the preparation method according to any one of claims 1 to 8.

10. Application of the modified lignin-derived hard carbon negative electrode material according to claim 9 in the field of batteries.

Citation Information

Patent Citations

  • Hard carbon microspheres with tunable morphology and pore structure, their preparation methods and applications

    CN110921647B

  • Hard carbon material, preparation method thereof and sodium ion battery

    CN116514105A

  • Lignin-based hard carbon / carbon nanotube composite material and preparation method and application thereof in negative electrode materials of lithium ion batteries

    CN107959006A

  • High-rate hard carbon negative electrode material and preparation method and application thereof

    CN115849332A

  • High-dispersion lignin-derived Ru in-situ N-doped carbon material as well as preparation method and application thereof