Boron-doped magnetic porous carbon wave-absorbing material and preparation method thereof

By compounding porous carbon materials with iron and its oxides, and incorporating boron atoms during the carbonization process, the problems of poor impedance matching and weak absorption intensity of traditional absorbing materials are solved, achieving strong absorption, wide frequency band and low density. Absorbing materials meet the development needs of "thin, light, wide and strong" absorbing materials.

CN118723971AActive Publication Date: 2024-10-01HARBIN ENG UNIV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410730429.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-01
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

Traditional absorbing materials cannot meet the current development needs for "thin, light, wide, and strong" absorbing materials. Poor impedance matching, weak absorption strength, and high density limit their further development in absorbing materials.

Method used

Porous carbon materials are combined with iron and its oxides to synthesize iron-containing hyper-crosslinked porous polymers through Friedel-Crafts reaction, and boron atoms are incorporated during the carbonization process to adjust the electronic structure of the carbon lattice and enhance polarization loss. , improve the conductivity and magnetic loss of the material.

Benefits of technology

It achieves excellent performance of strong absorption and wide frequency band, while significantly reducing the density of the material. The preparation method is simple and the cost is low, meeting the needs of lightweight, broadband and efficient absorbing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723971A_ABST
    Figure CN118723971A_ABST
Patent Text Reader

Abstract

The invention discloses a boron-doped magnetic porous carbon wave-absorbing material and a preparation method thereof, and belongs to the technical field of electromagnetic wave absorbing materials. The method comprises the following steps: synthesizing an iron-containing super-crosslinked porous polymer through a Friedel-Crafts reaction, uniformly mixing a boron doping agent with the iron-containing super-crosslinked porous polymer, and carrying out high-temperature carbonization in a tubular furnace to obtain the boron-doped magnetic porous carbon wave-absorbing material. The preparation method is simple and low in cost, the porous structure increases the reflection path of electromagnetic waves, the magnetic component provides magnetic loss and forms a heterogeneous interface with the carbon component to provide interface polarization, the doped boron atoms improve the dipole polarization capability of the material, and through the combined action of the loss mechanisms, the excellent performance of strong absorption and wide frequency band is achieved, and the application prospect is wide. Meanwhile, the porous structure remarkably reduces the density of the material, and a new thought is provided for preparation of light, broadband and efficient wave-absorbing materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electromagnetic wave absorbing materials, and relates to a lightweight porous carbon absorbing material and a preparation method thereof, and specifically relates to a boron-doped magnetic porous carbon absorbing material and a preparation method thereof. Background Art

[0002] Electromagnetic energy propagates in the form of waves to distant places without returning to the source of the waves, which is called electromagnetic radiation. Natural phenomena such as atmospheric lightning, cosmic rays, solar and earth thermal radiation can cause natural electromagnetic radiation. Production-type electronic and electrical equipment and various life-type electronic products will generate artificial electromagnetic radiation when they are working. The disordered and ultra-high intensity radiation of these electromagnetic waves will cause electromagnetic wave pollution. Electromagnetic wave radiation has become a new pollution source with greater harm after water pollution, air pollution and noise pollution. It not only affects normal communications, but also directly threatens human health. It has become a hot issue of concern to society and the scientific community. Electromagnetic wave absorbing material is a functional material that can convert the incident electromagnetic wave energy into heat energy or other forms of energy through electromagnetic loss and consume it. It is a key material to solve electromagnetic radiation pollution.

[0003] Traditional absorbing materials are mainly divided into two types according to the loss mechanism: electrical loss and magnetic loss: (1) Electrical loss absorbing materials can be further divided into dielectric absorbing materials and resistive absorbing materials: Dielectric absorbing materials represented by barium titanate and silicon carbide have an absorption mechanism in which the medium is repeatedly polarized so that electromagnetic energy is converted into heat energy and dissipated; resistive absorbing materials represented by carbon fiber materials and carbon nanotubes have a mechanism in which the conductive carriers inside the material move in a directional manner under the action of the electric field to form a conduction current, causing the electromagnetic energy to be lost in the form of heat energy. (2) Magnetic loss absorbing materials represented by ferrite and carbonyl iron achieve the purpose of absorbing waves by converting electromagnetic energy into heat energy during the magnetization and demagnetization process of magnetic materials.

[0004] Electrically lossy absorbing materials are widely used in the preparation of lightweight absorbing materials due to their low density, but their disadvantages are poor impedance matching and weak absorption intensity. Although magnetically lossy absorbing materials have the advantages of low cost, easy preparation, and strong absorption, their high density and narrow absorption band also limit their further development in absorbing materials. In view of the above problems, traditional absorbing materials cannot meet the current development requirements of "thin, light, wide, and strong" absorbing materials. The development of new absorbers is increasingly inclined to obtain composite absorbers by constructing multi-component complex structures. Summary of the invention

[0005] The purpose of the present invention is to solve the problem that traditional absorbing materials cannot meet the current development requirements of "thin, light, wide and strong" absorbing materials, and to provide a boron-doped magnetic porous carbon absorbing material and a preparation method thereof. The prepared absorbing material has multiple loss mechanisms, and also has the advantages of low density, wide absorption bandwidth, simple preparation method and low raw material price.

[0006] The present invention combines porous carbon materials with iron and its oxides to enhance impedance matching, allowing as many electromagnetic waves as possible to enter the material. At the same time, boron atoms are doped into the carbon lattice to adjust the electronic structure of adjacent carbon atoms and enhance polarization loss. The coordination between the various loss mechanisms within the composite material greatly improves the attenuation capability of incident electromagnetic waves.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing a boron-doped magnetic porous carbon wave absorbing material, wherein an iron-containing super-crosslinked porous polymer is used as a porous carbon skeleton precursor, and boron is doped into the carbon lattice during carbonization.

[0009] Furthermore, the method comprises the following steps:

[0010] Step 1: Synthesis of iron-containing hyper-crosslinked porous polymer by Friedel-Crafts reaction: Under nitrogen conditions, monomers, crosslinking agents, and catalyst anhydrous ferric chloride are mixed in a solvent to carry out Friedel-Crafts reaction to prepare an iron-containing hyper-crosslinked porous polymer;

[0011] Step 2: Preparation of boron-doped magnetic porous carbon absorbing material by high-temperature carbonization: Under nitrogen conditions, the boron dopant and the iron-containing hyper-crosslinked porous polymer are evenly mixed and then placed in a tubular furnace for high-temperature carbonization to obtain a boron-doped magnetic porous carbon absorbing material.

[0012] Furthermore, the step one is specifically as follows: under nitrogen conditions, 1 to 3 molar parts of monomer, 1 to 4 molar parts of cross-linking agent, and 2 to 10 molar parts of catalyst anhydrous ferric chloride are dissolved in a reaction solvent, and the reaction temperature is divided into three stages: the first temperature section is 30 to 50°C, the second temperature section is 50 to 70°C, and the third temperature section is 70 to 90°C, and each temperature section reacts for 20 to 28 hours; after the reaction is completed, suction filtration is performed, and the filter cake is dried in a vacuum oven at 60°C for 6 to 8 hours to obtain an iron-containing hyper-cross-linked porous polymer.

[0013] Furthermore, in step 1, the monomer is one or more of naphthalene, anthracene, phenanthrene, pyrene, biphenyl, terphenyl, o-diphenylbenzene, triphenylbenzene, and tetraphenylmethane; the cross-linking agent is one or more of dimethoxymethane, 1,3,5-tris(chloromethyl)benzene, 1,3,5-tris(chloromethyl)-2,4,6-trimethylbenzene, p-dichlorobenzyl, and biphenyl dichlorobenzyl; and the solvent is one of 1,2-dichloroethane and carbon tetrachloride.

[0014] Furthermore, the step 2 is specifically as follows: dispersing 1 to 4 parts by mass of an iron-containing hyper-crosslinked porous polymer and 0.5 to 4 parts of a boron dopant in a liquid medium, stirring at room temperature for 30 to 40 minutes to mix them evenly, collecting by centrifugation, and drying in a vacuum oven at 60°C for 6 to 8 hours; transferring the dry powder to a porcelain boat and placing it in a tubular furnace, setting the heating rate to 3 to 8°C / min, the carbonization temperature to 650 to 850°C, and the carbonization time to 1 to 3 hours under nitrogen conditions to obtain a boron-doped magnetic porous carbon absorbing material.

[0015] Furthermore, the boron dopant is one or more of elemental boron, boric acid, and boron trioxide.

[0016] Furthermore, the liquid medium is one or more of deionized water, anhydrous ethanol, and anhydrous methanol.

[0017] A boron-doped magnetic porous carbon wave absorbing material prepared by the above preparation method.

[0018] The beneficial effects of the present invention relative to the prior art are as follows: the present invention utilizes Friedel-Crafts reaction to synthesize a hyper-crosslinked polymer with a stable porous structure, and ferric chloride can not only be used as a highly active Lewis acid catalyst to promote the polymerization of monomers, but also as an iron source in the carbonization process. The iron-containing hyper-crosslinked porous polymer is mixed evenly with a boron dopant and then carbonized at high temperature, and the hyper-crosslinked porous skeleton is sintered into a porous carbon structure. The graphite carbon in the porous carbon structure increases the conductivity of the material and improves the conductive loss. At the same time, the porous structure is not only conducive to multiple reflections and interface polarization, but also can significantly reduce the density of the material; boron atoms have an atomic radius similar to that of carbon and can easily enter the carbon lattice. The doping of boron atoms adjusts the electronic structure of adjacent carbon atoms and enhances dipole polarization; trivalent iron is converted into elemental iron and its oxide, providing magnetic loss, and redistributing the charge at the interface with carbon, causing interface polarization. In summary, the preparation method of the present invention is simple and low in cost. By improving the coordination between multiple loss mechanisms, the excellent performance of strong absorption and broadband is achieved, while the density of the material is significantly reduced, and it has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1is a nitrogen adsorption-desorption curve diagram of the boron-doped magnetic porous carbon absorbing material of Example 1 of the present invention;

[0020] Figure 2 is a pore size distribution curve diagram of the boron-doped magnetic porous carbon absorbing material of Example 1 of the present invention;

[0021] Figure 3 is a scanning electron microscope image of the boron-doped magnetic porous carbon absorbing material of Example 1 of the present invention;

[0022] Figure 4 is a reflection loss curve of the boron-doped magnetic porous carbon absorbing material of Example 1 of the present invention;

[0023] Figure 5 is a reflection loss curve of the boron-doped magnetic porous carbon absorbing material of Example 2 of the present invention;

[0024] Figure 6 is a reflection loss curve of the boron-doped magnetic porous carbon absorbing material of Example 3 of the present invention;

[0025] Figure 7 is a reflection loss curve of the boron-doped magnetic porous carbon absorbing material of Example 4 of the present invention;

[0026] Figure 8 is a reflection loss curve of the boron-doped magnetic porous carbon absorbing material of Example 5 of the present invention;

[0027] Fig. 9 It is a reflection loss curve diagram of the boron-doped magnetic porous carbon absorbing material of Example 6 of the present invention. DETAILED DESCRIPTION

[0028] The present invention will be described in detail below in conjunction with the accompanying drawings.

[0029] The present invention and its implementation methods are described below, which are not restrictive and the actual implementation methods are not limited thereto. In short, if ordinary technicians in the field are inspired by it and design structural methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

[0030] The preparation method of the present invention is simple and has low cost. The porous structure increases the reflection path of electromagnetic waves. The magnetic component provides magnetic loss and forms a heterogeneous interface with the carbon component to provide interface polarization. The doped boron atoms improve the dipole polarization ability of the material. Through the joint action of these loss mechanisms, the excellent performance of strong absorption and wide bandwidth is achieved. At the same time, the porous structure significantly reduces the density of the material, providing a new idea for the preparation of lightweight, broadband and high-efficiency absorbing materials.

[0031] Embodiment 1:

[0032] Step 1: Under nitrogen conditions, 1 part of phenanthrene, 3 parts of benzyl dichloride, and 2 parts of anhydrous ferric chloride are dissolved in 80 ml of 1,2-dichloroethane, the reaction system is heated to a first temperature section of 45° C., and reacted at this temperature section for 20 hours, the reaction system is heated to a second temperature section of 65° C., and reacted at this temperature section for 20 hours, and the reaction system is further heated to a third temperature section of 80° C., and reacted at this temperature section for 20 hours; after the reaction is completed, suction filtration is performed, and the filter cake is dried in a vacuum oven at 60° C. for 6 to 8 hours to obtain an iron-containing hyper-crosslinked porous polymer.

[0033] Step 2: Disperse 1 part by weight of an iron-containing hyper-crosslinked porous polymer and 2 parts of boric acid in anhydrous ethanol, stir at room temperature for 30 to 40 minutes to mix them evenly, collect them by centrifugation, and dry them in a vacuum oven at 60°C for 6 to 8 hours; transfer the dry powder to a porcelain boat and put it into a tubular furnace, set the heating rate to 4°C / min, the carbonization temperature to 720°C, and the carbonization time to 3 hours under nitrogen conditions to obtain a boron-doped magnetic porous carbon absorbing material.

[0034] Figure 1 This is a nitrogen adsorption-desorption curve of the boron-doped magnetic porous carbon absorbing material in Example 1. According to the IUPAC classification, Figure 1 It is a typical type IV isotherm, and an obvious hysteresis loop appears in the medium pressure region, indicating that it has mesoporous properties. In addition, the specific surface area reaches 597.88m 2 / g, BJH pore volume is 0.59cm 3 / g. Figure 2 This is a pore size distribution curve of the boron-doped magnetic porous carbon absorbing material of Example 1. The pore size is mainly distributed at 3.93 nm, which proves that the sample of Example 1 has a porous structure. Figure 3 This is a scanning electron microscope image of the boron-doped magnetic porous carbon absorbing material of Example 1. It can be seen that the carbonized sample presents a flower-like morphology, and it can be clearly seen that the sample has abundant pores. The porous structure not only provides a large specific surface area and total pore volume for the composite material, but also generates multiple reflections and scattering to dissipate energy, converting microwave energy into heat energy or other energy during long-term propagation. In addition, the porous structure also helps to reduce the density of the absorbing material. Figure 4 This is the reflection loss diagram of the boron-doped magnetic porous carbon in Example 1. When the filling ratio is 30%, it has the best electromagnetic wave absorption effect when the matching thickness is 2.40 mm, the minimum reflection loss is -50.54 dB, the effective absorption frequency range is 10.64 to 18.00 GHz, and the effective absorption bandwidth is 7.36 GHz.

[0035] Embodiment 2:

[0036] Step 1: Under nitrogen conditions, 2 parts of anthracene, 1 part of biphenyl dichlorobenzyl, and 3 parts of anhydrous ferric chloride are dissolved in 80 ml of 1,2-dichloroethane, the reaction system is heated to a first temperature section of 48° C., reacted at this temperature section for 22 hours, the reaction system is heated to a second temperature section of 68° C., reacted at this temperature section for 22 hours, and the reaction system is continuously heated to a third temperature section of 75° C., reacted at this temperature section for 26 hours; after the reaction is completed, suction filtration is performed, and the filter cake is dried in a vacuum oven at 60° C. for 6 to 8 hours to obtain an iron-containing hyper-crosslinked porous polymer.

[0037] Step 2: Disperse 1 part by weight of an iron-containing hyper-crosslinked porous polymer and 1 part of boric acid in deionized water, stir at room temperature for 30 to 40 minutes to mix them evenly, collect them by centrifugation, and dry them in a vacuum oven at 60°C for 6 to 8 hours; transfer the dry powder to a porcelain boat and place it in a tubular furnace, set the heating rate to 4°C / min, the carbonization temperature to 720°C, and the carbonization time to 3 hours under nitrogen conditions to obtain a boron-doped magnetic porous carbon absorbing material.

[0038] Figure 5 This is the reflection loss diagram of the boron-doped magnetic porous carbon of Example 2. When the filling ratio is 30%, it has the best electromagnetic wave absorption effect when the matching thickness is 3.50 mm, the minimum reflection loss is -47.51 dB, the effective absorption frequency range is 11.52 to 18.00 GHz, and the effective absorption bandwidth is 6.48 GHz.

[0039] Embodiment 3:

[0040] Step 1: Under nitrogen conditions, 1 part of triphenylbenzene, 2 parts of biphenyl dichlorobenzyl, and 4 parts of anhydrous ferric chloride are dissolved in 80 ml of 1,2-dichloroethane, the reaction system is heated to a first temperature section of 45° C., and reacted at this temperature section for 20 hours, the reaction system is heated to a second temperature section of 65° C., and reacted at this temperature section for 20 hours, and the reaction system is further heated to a third temperature section of 80° C., and reacted at this temperature section for 20 hours; after the reaction is completed, suction filtration is performed, and the filter cake is dried in a vacuum oven at 60° C. for 6 to 8 hours to obtain an iron-containing hyper-crosslinked porous polymer.

[0041] Step 2: Disperse 1 part by weight of an iron-containing hyper-crosslinked porous polymer and 3 parts of boron trioxide in deionized water, stir at room temperature for 30 to 40 minutes to mix them evenly, collect them by centrifugation, and dry them in a vacuum oven at 60°C for 6 to 8 hours; transfer the dry powder to a porcelain boat and place it in a tubular furnace, set the heating rate to 6°C / min, the carbonization temperature to 750°C, and the carbonization time to 2 hours under nitrogen conditions to obtain a boron-doped magnetic porous carbon absorbing material.

[0042] Figure 6 This is the reflection loss diagram of the boron-doped magnetic porous carbon in Example 3. When the filling ratio is 30%, it has the best electromagnetic wave absorption effect when the matching thickness is 2.20 mm, the minimum reflection loss is -38.68 dB, the effective absorption frequency range is 12.00 to 18.00 GHz, and the effective absorption bandwidth is 6.60 GHz.

[0043] Embodiment 4:

[0044] Step 1: Under nitrogen conditions, 2 parts of biphenyl, 1 part of dimethoxymethane, and 5 parts of anhydrous ferric chloride are dissolved in 80 ml of carbon tetrachloride, the reaction system is heated to a first temperature section of 40° C., and the reaction is carried out at this temperature section for 20 hours, the reaction system is heated to a second temperature section of 65° C., and the reaction is carried out at this temperature section for 25 hours, and the reaction system is further heated to a third temperature section of 75° C., and the reaction is carried out at this temperature section for 20 hours; after the reaction is completed, suction filtration is performed, and the filter cake is dried in a vacuum oven at 60° C. for 6 to 8 hours to obtain an iron-containing hyper-crosslinked porous polymer.

[0045] Step 2: Disperse 1 part by weight of an iron-containing hyper-crosslinked porous polymer and 1 part of elemental boron in anhydrous methanol, stir at room temperature for 30 to 40 minutes to mix them evenly, collect them by centrifugation, and dry them in a vacuum oven at 60°C for 6 to 8 hours; transfer the dry powder to a porcelain boat and put it into a tubular furnace, set the heating rate to 6°C / min, the carbonization temperature to 750°C, and the carbonization time to 2 hours under nitrogen conditions to obtain a boron-doped magnetic porous carbon absorbing material.

[0046] Figure 7 This is the reflection loss diagram of the boron-doped magnetic porous carbon of Example 4. When the filling ratio is 30%, it has the best electromagnetic wave absorption effect when the matching thickness is 3.50 mm, the minimum reflection loss is -38.70 dB, the effective absorption frequency range is 11.52 to 18.00 GHz, and the effective absorption bandwidth is 6.48 GHz.

[0047] Embodiment 5:

[0048] Step 1: Under nitrogen conditions, 2 parts of tetraphenylmethane, 1 part of 1,3,5-tris(chloromethyl)-2,4,6-trimethylbenzene, and 6 parts of anhydrous ferric chloride are dissolved in 100 ml of 1,2-dichloroethane, the reaction system is heated to a first temperature section of 40° C., reacted in this temperature section for 20 hours, the reaction system is heated to a second temperature section of 65° C., reacted in this temperature section for 24 hours, and the reaction system is continuously heated to a third temperature section of 75° C., reacted in this temperature section for 22 hours; after the reaction is completed, suction filtration is performed, and the filter cake is dried in a vacuum oven at 60° C. for 6 to 8 hours to obtain an iron-containing hyper-crosslinked porous polymer.

[0049] Step 2: Disperse 1 part by weight of an iron-containing hyper-crosslinked porous polymer and 1.5 parts of elemental boron in anhydrous methanol, stir at room temperature for 30 to 40 minutes to mix them evenly, collect them by centrifugation, and dry them in a vacuum oven at 60°C for 6 to 8 hours; transfer the dry powder to a porcelain boat and put it into a tubular furnace, set the heating rate to 6°C / min, the carbonization temperature to 720°C, and the carbonization time to 2 hours under nitrogen conditions to obtain a boron-doped magnetic porous carbon absorbing material.

[0050] Figure 8 This is the reflection loss diagram of the boron-doped magnetic porous carbon of Example 5. When the filling ratio is 30%, it has the best electromagnetic wave absorption effect when the matching thickness is 2.20 mm, the minimum reflection loss is -38.67 dB, the effective absorption frequency range is 12.00 to 18.00 GHz, and the effective absorption bandwidth is 6.00 GHz.

[0051] Embodiment 6:

[0052] Step 1: Under nitrogen conditions, 2 parts of o-diphenylbenzene, 1 part of dimethoxymethane, and 10 parts of anhydrous ferric chloride are dissolved in 90 ml of carbon tetrachloride, the reaction system is heated to a first temperature section of 40°C, and the reaction is carried out at this temperature section for 20 hours, the reaction system is heated to a second temperature section of 65°C, and the reaction is carried out at this temperature section for 20 hours, and the reaction system is further heated to a third temperature section of 75°C, and the reaction is carried out at this temperature section for 24 hours; after the reaction is completed, suction filtration is performed, and the filter cake is dried in a vacuum oven at 60°C for 6 to 8 hours to obtain an iron-containing hyper-crosslinked porous polymer.

[0053] Step 2: Disperse 1 part by weight of an iron-containing hyper-crosslinked porous polymer and 2.5 parts of elemental boron in anhydrous methanol, stir at room temperature for 30 to 40 minutes to mix them evenly, collect them by centrifugation, and dry them in a vacuum oven at 60°C for 6 to 8 hours; transfer the dry powder to a porcelain boat and place it in a tubular furnace, set the heating rate to 5°C / min, the carbonization temperature to 700°C, and the carbonization time to 2 hours under nitrogen conditions to obtain a boron-doped magnetic porous carbon absorbing material.

[0054] Fig. 9 This is the reflection loss diagram of the boron-doped magnetic porous carbon of Example 6. When the filling ratio is 30%, it has the best electromagnetic wave absorption effect when the matching thickness is 2.20 mm, the minimum reflection loss is -29.61 dB, the effective absorption frequency range is 12.24 to 18.00 GHz, and the effective absorption bandwidth is 5.76 GHz.

[0055] Table 1 summarizes the electromagnetic absorption performance of Examples 1-6. From the test results, it can be seen that the magnetic porous carbon lightweight absorbing material formed by using an iron-containing hyper-crosslinked porous polymer as a porous carbon skeleton precursor and incorporating boron into the carbon lattice during carbonization has excellent absorbing performance. Among them, Example 1 has the best comprehensive absorbing performance. When the filling ratio is 30%, it has a minimum reflection loss of -50.54dB and an effective absorption bandwidth of 7.36GHz. The sample has high absorption intensity, wide absorption bandwidth, low density, and thin matching thickness, which meets the current development requirements for absorbing materials to be "thin, light, wide, and strong".

[0056] Table 16 Electromagnetic wave absorption performance of samples in the examples

[0057]

Claims

1. A method for preparing a boron-doped magnetic porous carbon absorbing material, characterized in that: The method uses an iron-containing hyper-crosslinked porous polymer as a porous carbon skeleton precursor and incorporates boron into the carbon lattice during carbonization.

2. The method for preparing a boron-doped magnetic porous carbon absorbing material according to claim 1, characterized in that: The method comprises the following steps: Step 1: Synthesis of iron-containing hyper-crosslinked porous polymer by Friedel-Crafts reaction: Under nitrogen conditions, monomers, crosslinking agents, and catalyst anhydrous ferric chloride are mixed in a solvent to carry out Friedel-Crafts reaction to prepare an iron-containing hyper-crosslinked porous polymer; Step 2: Preparation of boron-doped magnetic porous carbon absorbing material by high-temperature carbonization: Under nitrogen conditions, the boron dopant and the iron-containing hyper-crosslinked porous polymer are evenly mixed and then placed in a tubular furnace for high-temperature carbonization to obtain a boron-doped magnetic porous carbon absorbing material.

3. The method for preparing a boron-doped magnetic porous carbon absorbing material according to claim 2, characterized in that: The step 1 is specifically as follows: under nitrogen conditions, 1 to 3 parts of monomers, 1 to 4 parts of cross-linking agents, and 2 to 10 parts of anhydrous ferric chloride as a catalyst are dissolved in a reaction solvent, and the reaction temperature is divided into three stages: the first temperature section is 30 to 50° C., the second temperature section is 50 to 70° C., and the third temperature section is 70 to 90° C., and each temperature section reacts for 20 to 28 hours; after the reaction is completed, suction filtration is performed, and the filter cake is dried in a vacuum oven at 60° C. for 6 to 8 hours to obtain an iron-containing hyper-cross-linked porous polymer.

4. The method for preparing a boron-doped magnetic porous carbon absorbing material according to claim 2 or 3, characterized in that: In step 1, the monomer is one or more of naphthalene, anthracene, phenanthrene, pyrene, biphenyl, terphenyl, o-diphenylbenzene, triphenylbenzene, and tetraphenylmethane; the cross-linking agent is one or more of dimethoxymethane, 1,3,5-tris(chloromethyl)benzene, 1,3,5-tris(chloromethyl)-2,4,6-trimethylbenzene, p-dichlorobenzyl, and biphenyl dichlorobenzyl; and the solvent is one of 1,2-dichloroethane and carbon tetrachloride.

5. The method for preparing a boron-doped magnetic porous carbon absorbing material according to claim 2, characterized in that: The step 2 is specifically as follows: dispersing 1 to 4 parts by weight of an iron-containing hyper-crosslinked porous polymer and 0.5 to 4 parts by weight of a boron dopant in a liquid medium, stirring at room temperature for 30 to 40 minutes to mix them evenly, collecting by centrifugation, and drying in a vacuum oven at 60° C. for 6 to 8 hours; transferring the dry powder into a porcelain boat and placing it in a tubular furnace, setting the heating rate to 3 to 8° C. / min, the carbonization temperature to 650 to 850° C., and the carbonization time to 1 to 3 hours under nitrogen conditions to obtain a boron-doped magnetic porous carbon absorbing material.

6. The method for preparing a boron-doped magnetic porous carbon absorbing material according to claim 2 or 5, characterized in that: The boron dopant is one or more of elemental boron, boric acid, and boron trioxide.

7. The method for preparing a boron-doped magnetic porous carbon absorbing material according to claim 5, characterized in that: The liquid medium is one or more of deionized water, anhydrous ethanol and anhydrous methanol.

8. A boron-doped magnetic porous carbon absorbing material prepared by the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Preparation method of graphene reinforced biomass porous carbon electromagnetic wave-absorbing material

    CN110467175A

  • Conductive polymer coated super-crosslinked porous polymer wave-absorbing agent and preparation method thereof

    CN117417526A

  • Asphalt Concrete Pavement Containing Wave Absorbing Material and Maintenance Process Thereof

    US20120027513A1