Preparation and application of cobalt-based MOF carbon wave-absorbing material
Through hydrothermal reaction and high-temperature annealing treatment of cobalt-based MOF materials, cobalt-based MOF carbon absorbing materials with multiple interfaces and channels were prepared, which solved the problem of insufficient performance of existing absorbing materials and achieved excellent electromagnetic wave absorption effects. Suitable for life and military monitoring fields.
Patent Information
- Application Number
- CN202410677962.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-29
AI Technical Summary
Existing absorbing materials have insufficient performance in practical applications, especially poor impedance matching and poor attenuation capabilities, which limit their application in the fields of daily life and military monitoring, and it is difficult for a single component material to achieve comprehensive performance.
Cobalt-based metal-organic framework (MOF) materials are prepared through hydrothermal reaction and high-temperature annealing treatment to form cobalt-based MOF carbon absorbing materials with multiple interfaces and pores, which utilize dielectric loss and interface relaxation effects to achieve electromagnetic wave absorption.
The prepared cobalt-based MOF carbon absorbing material shows excellent electromagnetic wave absorption performance. The material is lighter and has low density. The microstructure formed after annealing strengthens dipole polarization and conductive loss, achieving better absorption effect, especially at 700 The minimum reflection loss reaches -30.2dB at ℃.
Smart Images

Figure CN118723987A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electromagnetic wave absorbing materials, and in particular to the preparation and application of a cobalt-based MOF carbon absorbing material. Background Art
[0002] From radio broadcasting to mobile phone communications to satellite navigation, the use of electromagnetic waves has brought great convenience to human life, but at the same time, the electromagnetic radiation caused by redundant electromagnetic waves has also caused great harm to people's living environment and physical health. On the one hand, high-frequency electromagnetic waves will affect the normal operation of vehicles and factory machines. On the other hand, electromagnetic radiation will attack the human immune system and nervous system, especially infants and children. They are in the growth and development stage, and their cells and tissues are relatively fragile. Low-intensity electromagnetic waves will induce the occurrence of childhood leukemia and cause serious consequences to the body. In this context, microwave absorbing materials that can absorb and dissipate electromagnetic waves through their own absorbing properties or by constructing special structures have become a major research direction.
[0003] Traditional absorbing materials such as metal powder, ferrite, transition metal oxides and their sulfides, and carbon materials have shown excellent absorbing performance, but single-component materials often cannot fully demonstrate their performance. Even if their magnetic loss performance is excellent, their high density greatly limits the application and development of these materials in real life and military monitoring. Traditional carbon materials have a relatively narrow electromagnetic wave band that can be efficiently absorbed due to their poor impedance matching and poor attenuation constant. At present, excellent absorbing materials usually have the performance of "thin, light, wide, and strong", so we need to develop more promising composite materials.
[0004] Metal organic framework (MOF) is a new type of coordination compound with typical periodicity and network structure. The structure mainly includes organic ligands and metal nodes. The structure can be changed by controlling the ligand ratio and temperature conditions during the synthesis process in the experiment, which makes MOF material a popular precursor of absorbing materials. The magnetic absorbing material prepared by high temperature pyrolysis of metal organic framework shows good performance in the experiment. Therefore, the present invention achieves effective absorbing performance by processing a cobalt-based MOF material. Summary of the invention
[0005] In view of the above-mentioned technical problems existing in the prior art, the purpose of the present application is to provide a preparation and application of a cobalt-based MOF carbon absorbing material.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A method for preparing a cobalt-based MOF carbon absorbing material comprises the following steps: hydrothermal reaction of cobalt salt and citric acid to obtain a metal organic framework UTSA-16, and then high temperature annealing treatment is performed under the protection of an inert gas to obtain the cobalt-based MOF carbon absorbing material.
[0008] Furthermore, the molar ratio of the cobalt salt to the citric acid is 1:0.5-2, preferably 1:1.
[0009] The method for preparing a cobalt-based MOF carbon absorbing material specifically comprises the following steps:
[0010] 1) dissolving cobalt salt in water to form solution A;
[0011] 2) dissolving citric acid in an ethanol-water solvent and adding a strong base to neutralize the pH value of the solution to form solution B;
[0012] 3) adding solution A dropwise and slowly into solution B under stirring, transferring the resulting mixed solution into a reactor with a polytetrafluoroethylene liner, and setting a partition in the polytetrafluoroethylene liner to divide its internal space into 3-10 small spaces, sealing the reactor and transferring it to an oven for hydrothermal reaction; after the reaction, collecting the solid by centrifugation, washing, and drying, thereby obtaining UTSA-16 crystals;
[0013] 4) The fully dried UTSA-16 crystals are sent into a tubular furnace and subjected to high temperature annealing treatment under the protection of an inert gas to obtain the cobalt-based MOF carbon absorbing material.
[0014] Furthermore, in step 1), the concentration of cobalt salt in solution A is 0.1-1 mmol / mL, preferably 0.4-0.5 mmol / L.
[0015] Further, in step 2), the volume ratio of ethanol to water is 0.5-2.5:1, the strong base is KOH, the molar ratio of the strong base to citric acid is 2-4:1, preferably 3:1, and the concentration of citric acid in solution B is 0.1-1 mmol / mL, preferably 0.25-0.4 mmol / L.
[0016] Furthermore, in step 3), the temperature of the hydrothermal reaction is 100-130° C., preferably 110-120° C., and the time of the hydrothermal reaction is 24-60 h, preferably 40-48 h.
[0017] Further, in step 4), the inert gas is nitrogen, and the high temperature annealing operation is: heating to 600-800°C at a heating rate of 1°C / min-10°C / min, then keeping warm for 2-3h, and then cooling to room temperature at a rate of 1°C / min-10°C / min.
[0018] Furthermore, the heating rate is 4-5°C / min, the holding temperature is 650-700°C, and the cooling rate is 2-3°C / min.
[0019] The present invention also provides application of the cobalt-based MOF carbon absorbing material in microwave absorption.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The Co-based MOF carbon-derived absorbing material prepared by the present invention has excellent electromagnetic wave absorption performance. Through microscopic analysis and theoretical speculation, the absorption mechanism of the material is mainly dielectric loss. During the annealing process, the multiple interfaces and pores of the metal nanoparticle composite carbon-based material induce the interface relaxation effect. Under the action of an external electric field, the interface relaxation of the material is a major mechanism of electromagnetic wave absorption.
[0022] 2. The Co-based MOF carbon-derived absorbing material prepared by the present invention forms abundant heterogeneous interfaces and surface defects between the microscopic metal Co particles, graphite carbon and amorphous carbon formed after annealing, which further strengthens the dipole polarization and makes a great contribution to the dielectric loss.
[0023] 3. The Co-based MOF carbon-derived absorbing material prepared by the present invention forms a carbon skeleton after annealing, and the exposed Co metal provides a large conductivity loss, and the material is light, with a density of 0.1356 mg·mmol at room temperature. -1 In summary, the minimum RL value of this material reached -30.2dB under the conditions of annealing temperature of 700℃ and matching thickness of 4mm.
[0024] 4. The UTSA-16 precursor used in the present invention is prepared with cheap and low-toxic water and ethanol as solvents, and the preparation process is green and environmentally friendly. In this experiment, a "cross" polytetrafluoroethylene plate is used to insert the polytetrafluoroethylene liner, which increases the sites for the generation of crystal nuclei and greatly helps to improve the yield. By analogy, by increasing the surface area of the reactor, it is very promising for industrial mass synthesis. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the XRD pattern of the UTSA-16 crystal in step 1) of Example 1.
[0026] Figure 2 This is the SEM image of Co@C-600 in step 2) of Example 1.
[0027] Figure 3 This is a test diagram of the microwave absorption performance of Co@C-600 in Example 1.
[0028] Figure 4This is the SEM image of Co@C-700 of Example 2.
[0029] Figure 5 This is the EDS graph of Co@C-700 of Example 2.
[0030] Figure 6 This is a test diagram of the microwave absorption performance of Co@C-700 in Example 2.
[0031] Figure 7 This is the SEM image of Co@C-800 of Example 3.
[0032] Figure 8 This is a test diagram of the microwave absorption performance of Co@C-800 in Example 3. DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0034] Embodiment 1:
[0035] A cobalt-based MOF carbon absorbing material, the preparation steps of which are as follows:
[0036] 1) 0.4203g (2.0mmol) C6H8O7·H2O and 0.3366g (6.0mmol) KOH were completely dissolved in 5mL ethanol and 2mL deionized water, which was recorded as solution A; 0.4982g Co(OAc)2·4H2O was completely dissolved in 3mL deionized water, which was recorded as solution B. Solution B was then transferred to solution A and stirred at room temperature for 15 minutes to fully mix. The mixture was then added to a stainless steel reactor with a polytetrafluoroethylene liner, a "cross"-shaped polytetrafluoroethylene partition was added in the liner, and the internal space of the liner was evenly divided into 4 small spaces. The reactor was sealed and transferred to an oven and heated at 120°C for 48 hours. The product was centrifuged at 9000r / min for 8 minutes, and the purple crystals were collected and washed three times with mother liquor, and then washed three times with ethanol, and finally dried in a vacuum drying oven at 60°C for 6 hours to obtain fully dried UTSA-16 crystals, which were weighed, bottled, dried and stored. The mass of the dry sample synthesized by this method was 267.2 mg, and the yield was about 62.00%.
[0037] 2) The fully dried UTSA-16 crystals were placed in a tube furnace, heated to 600°C at a rate of 5°C / min in a N2 atmosphere, and kept at a constant temperature for 3 hours, and then slowly cooled to room temperature at a rate of 2°C / min. The resulting carbon product was named Co@C-600.
[0038] Performance Testing
[0039] 1) The XRD pattern of the UTSA-16 crystal in step 1) of Example 1 is as follows Figure 1 As shown, the SEM image of Co@C-600 in step 2) of Example 1 is as follows Figure 2 shown.
[0040] Depend on Figure 1 It can be seen that characteristic peaks appear at 11.3°, 13.8°, 21.3° and 28.4°, respectively, which is consistent with the PDF card information of UTSA-16 crystal.
[0041] Depend on Figure 2 It can be seen that after calcination at 600°C, spherical protrusions are formed on the surface, which makes Co@C-600 rougher. At the same time, it can be observed that the microscopic crystal form of Co@C-600 is difficult to observe, and only some regular crystal shapes are presented on the edges.
[0042] 2) This article uses Agilent PNAN5234A vector network analyzer to test the electromagnetic parameters of the sample such as complex dielectric constant and complex magnetic permeability (frequency range: 2-18GHz). The coaxial method test sample preparation process is as follows: 1. Weigh the sample to be tested and mix it with paraffin (the mass fraction of the sample to be tested in the mixture is 30wt%), dissolve it in n-hexane solution, and stir and ultrasonicate to make it evenly dispersed. 2. Place the solution in a 75°C water bath and stir with a glass rod to evaporate the n-hexane in the solution to obtain a uniform sample powder wrapped in paraffin. 3. Put the powder into a mold and use a tablet press to press it into a ring-shaped sample (sample size: inner diameter 3mm, outer diameter 7mm, thickness 3mm). Obtain the following Figure 3 Wave absorption performance data graph.
[0043] Depend on Figure 3 It can be seen that Co@C-600 has effective absorption in the Ku band, and the overall RL peak weakens with the increase of thickness. When the thickness is 1.5 mm, the minimum reflection loss (RL) of Co@C-600 at the frequency of 16.9 GHz is min ) is -23.2dB. When the thickness is 2mm, the EAB of Co@C-600 reaches 3.1GHz (13.9-17.0GHz), showing good absorption performance in the high-frequency band.
[0044] Embodiment 2:
[0045] A cobalt-based MOF carbon absorbing material, the preparation steps of which are as follows:
[0046] 1) 0.4203g C6H8O7·H2O and 0.3366g KOH were completely dissolved in a solvent of 5mL ethanol and 2mL deionized water, which was recorded as solution A; 0.4982g Co(OAc)2·4H2O was completely dissolved in 3mL deionized water, which was recorded as solution B. Solution B was then transferred to solution A and stirred at room temperature for 15 minutes to fully mix. The mixture was then added to a stainless steel reactor with a polytetrafluoroethylene liner, a "cross"-shaped polytetrafluoroethylene partition was added to the liner, and the internal space of the liner was evenly divided into 4 small spaces. The reactor was sealed and transferred to an oven and heated at 120°C for 48 hours. The product was centrifuged at a speed of 9000r / min for 8 minutes, and the purple crystals were collected and washed three times with the mother liquor, and then washed three times with ethanol, and finally dried in a vacuum drying oven at 60°C for 6 hours.
[0047] 2) Place the fully dried UTSA-16 crystals into a tube furnace, heat it to 700°C at a rate of 5°C / min in a N2 atmosphere, and keep it there for 3 hours, then slowly cool it down to room temperature at a rate of 2°C / min. The resulting carbon product is named Co@C-700, and the density of Co@C-700 material at room temperature is 0.1356 mg·mmol -1 .
[0048] Performance Testing
[0049] 1) The SEM image of Co@C-700 in step 2) of Example 2 is as follows Figure 4 As shown, the EDS image of Co@C-700 in step 2) of Example 2 is as follows Figure 5 shown.
[0050] exist Figure 4 A large number of broken structures were found, and many carbon microspheres were formed on the surface. Unlike the structure of Co@C-600 prepared at 600°C, many regular crystal structures were found in the microstructure of Co@C-700. As shown in the figure, the crystal is generally octahedral, with a rhombus shape on the side, about 5μm in size and 2μm in thickness, and some carbon spheres are also grown on the surface.
[0051] Depend on Figure 5It can be seen that the Co and C of Co@C-700 are generally uniform, but Co is relatively concentrated, which indicates that during the calcination, along with the collapse of UTSA-16, the metal Co did not remain in place, but because of the capillary effect of the pores, the position changed, resulting in the formation of complex structures such as heterogeneous interfaces, which not only destroyed the original ordered structure and formed many irregular fragmented Co@C, but also indirectly enhanced the interface polarization effect. In addition, we can observe that C, O, and Co are evenly distributed throughout the EDS image, and are successfully doped with the chemical bonds of UTSA-16 during the calcination process. The defects formed by C on the surface of Co@C-700 can also enhance the ability of interface polarization.
[0052] 2) The detection method of the wave absorption performance is consistent with that in Example 1. The obtained wave absorption performance data is shown in the figure Figure 6 shown.
[0053] Depend on Figure 6 The Co@C-700 material has better performance and shows strong absorption in the low-frequency band. As the thickness increases, its RL value also increases. At a thickness of 4mm, the minimum RL value reaches -30.2dB, while the EAB decreases accordingly. The maximum EAB almost covers the entire Ku band when the thickness is 2.5mm. Interestingly, Co@C-700 shows a wide EAB in the high-frequency band under low thickness conditions, and a strong RL value in the medium and low frequency bands when the thickness is high.
[0054] Example 3
[0055] A cobalt-based MOF carbon absorbing material, the preparation steps of which are as follows:
[0056] 1) 0.4203g C6H8O7·H2O and 0.3366g KOH were completely dissolved in a solvent of 5mL ethanol and 2mL deionized water, which was recorded as solution A; 0.4982g Co(OAc)2·4H2O was completely dissolved in 3mL deionized water, which was recorded as solution B. Solution B was then transferred to solution A and stirred at room temperature for 15 minutes to fully mix. The mixture was then added to a stainless steel reactor with a polytetrafluoroethylene liner, a "cross"-shaped polytetrafluoroethylene partition was added to the liner, and the internal space of the liner was evenly divided into 4 small spaces. The reactor was sealed and transferred to an oven and heated at 120°C for 48 hours. The product was centrifuged at a speed of 9000r / min for 8 minutes, and the purple crystals were collected and washed three times with the mother liquor, and then washed three times with ethanol, and finally dried in a vacuum drying oven at 60°C for 6 hours.
[0057] 2) The fully dried UTSA-16 crystals were placed in a tube furnace, heated to 800°C at a rate of 5°C / min in a N2 atmosphere, and maintained for 3 hours, then slowly cooled to room temperature at a rate of 2°C / min. The resulting carbon product was named Co@C-800.
[0058] Performance Testing
[0059] 1) The SEM image of Co@C-800 in step 2) of Example 3 is as follows Figure 7 shown.
[0060] Depend on Figure 7 It can be seen that there is no obvious crystal structure on Co@C-800. Similar to Co@C-600, the overall agglomeration phenomenon is serious. Although carbon balls of a certain scale are formed on the surface, there are no obvious pores and the overall density is relatively large.
[0061] 2) According to the wave absorption performance test steps in Example 1, the wave absorption performance data diagram of Example 3 is obtained, as shown in FIG. Figure 8 shown.
[0062] Depend on Figure 8 It can be seen that when the temperature reaches 800℃, the RL value of Co@C-800 stabilizes at around -5dB, and the minimum is only -8dB, and no effective absorption occurs at all thicknesses. The attenuation ability and impedance matching of this material are both poor. According to the microstructure, it can be seen that the agglomeration effect at high temperature seriously affects the impedance matching effect, which greatly weakens the material's ability to dissipate electromagnetic waves.
[0063] In summary, it can be concluded that UTSA-16 / C calcined at 700°C exhibits strong absorbing performance. The minimum RL value reaches -30.2dB at a thickness of 4mm, while the EAB decreases accordingly. The maximum EAB almost covers the entire Ku segment when the thickness is 2.5mm.
[0064] Example 4
[0065] An iron-based MOF carbon absorbing material, the preparation steps of which are as follows:
[0066] 0.4203g C6H8O7·H2O and 0.3366g KOH were completely dissolved in 5mL ethanol and 2mL deionized water, which was recorded as solution A; 0.3819g Fe(OAc)3 was completely dissolved in 3mL deionized water, which was recorded as solution B. Solution B was then transferred to solution A and stirred at room temperature for 15 minutes to fully mix. The mixture was then added to a stainless steel reactor with a polytetrafluoroethylene liner, and a "cross" polytetrafluoroethylene partition was added to the liner to divide the internal space of the liner into 4 small spaces. The reactor was sealed and transferred to an oven and heated at 120°C for 48 hours. The product was centrifuged at a speed of 9000r / min for 8 minutes, washed three times with ethanol, and finally dried at 60°C in a vacuum drying oven for 6 hours.
[0067] According to the detection, the material after washing did not present a crystal particle morphology similar to that of Example 1, Example 2, and Example 3, but a block structure, so the iron-based MOF precursor of Example 4 did not achieve a good structure.
[0068] Example 5
[0069] An iron-cobalt-based binary MOF carbon absorbing material, the preparation steps of which are as follows:
[0070] 0.4203g C6H8O7·H2O and 0.3366g KOH were completely dissolved in a solvent of 5mL ethanol and 2mL deionized water, which was recorded as solution A; 0.2491g Co(OAc)2·4H2O and 0.1909g Fe(OAc)3 were completely dissolved in 3mL deionized water, which was recorded as solution B. Solution B was then transferred to solution A and stirred at room temperature for 15 minutes to fully mix. The mixture was then added to a stainless steel reactor with a polytetrafluoroethylene liner, and a "cross" polytetrafluoroethylene partition was added to the liner to divide the internal space of the liner into 4 small spaces. The reactor was sealed and transferred to an oven and heated at 120°C for 48 hours. The product was centrifuged at a speed of 9000r / min for 8 minutes, washed three times with ethanol, and finally dried at 60°C in a vacuum drying oven for 6 hours.
[0071] According to the test, the material did not present the crystal particle morphology similar to that of Example 1, Example 2, and Example 3 after washing, and did not form an effective crystalline structure. Therefore, the iron-cobalt-based binary MOF precursor of Example 5 did not achieve a good structure.
[0072] Example 6
[0073] A cobalt-based MOF carbon absorbing material, the preparation steps of which are as follows:
[0074] 0.1801g H2C2O4 and 0.2244g KOH were completely dissolved in a solvent of 5mL ethanol and 2mL deionized water, which was recorded as solution A; 0.4982g Co(OAc)2·4H2O was completely dissolved in 3mL deionized water, which was recorded as solution B. Solution B was then transferred to solution A and stirred at room temperature for 15 minutes to fully mix. The mixture was then added to a stainless steel reactor with a polytetrafluoroethylene liner, and a "cross" polytetrafluoroethylene partition was added to the liner to divide the internal space of the liner into 4 small spaces. The reactor was sealed and transferred to an oven and heated at 120°C for 48 hours. The product was centrifuged at a speed of 9000r / min for 8 minutes, washed three times with ethanol, and finally dried at 60°C in a vacuum drying oven for 6 hours. According to the test, the material after washing did not present a crystal particle morphology similar to that of Example 1, Example 2, and Example 3, but a powder-like structure, so the cobalt-based MOF precursor of Example 6 did not achieve a good structure.
[0075] The contents described in this specification are merely an enumeration of implementation forms of the inventive concept, and the protection scope of the present invention should not be regarded as being limited to the specific forms described in the embodiments.
Claims
1. A method for preparing a cobalt-based MOF carbon absorbing material, characterized in that The cobalt salt and citric acid are subjected to a hydrothermal reaction to obtain the metal organic framework UTSA-16, which is then subjected to a high temperature annealing treatment under the protection of an inert gas to obtain the cobalt-based MOF carbon absorbing material.
2. The method for preparing a cobalt-based MOF carbon absorbing material according to claim 1, characterized in that The molar ratio of the cobalt salt to the citric acid is 1:0.5-2, preferably 1:
1.
3. The method for preparing a cobalt-based MOF carbon absorbing material according to claim 1, characterized in that The specific steps include: 1) Dissolve cobalt salt in water to form solution A; 2) Dissolve citric acid in an ethanol-water solvent and add a strong base to neutralize the pH value of the solution to form solution B; 3) Solution A is slowly added dropwise to solution B under stirring, and the resulting mixed solution is transferred to a reactor with a polytetrafluoroethylene liner, and a partition is set in the polytetrafluoroethylene liner to divide its internal space into 3-10 small spaces, and the reactor is sealed and transferred to an oven for hydrothermal reaction; after the reaction is completed, the solid is collected by centrifugation, washed, and dried to obtain UTSA-16 crystals; 4) The fully dried UTSA-16 crystals are sent into a tubular furnace and annealed at high temperature under the protection of an inert gas to obtain the cobalt-based MOF carbon absorbing material.
4. The method for preparing a cobalt-based MOF carbon absorbing material according to claim 3, characterized in that In step 1), the concentration of cobalt salt in solution A is 0.1-1 mmol / mL, preferably 0.4-0.5 mmol / L.
5. The method for preparing a cobalt-based MOF carbon absorbing material according to claim 3, characterized in that In step 2), the volume ratio of ethanol to water is 0.5-2.5:1, the strong base is KOH, the molar ratio of the strong base to citric acid is 2-4:1, preferably 3:1, and the concentration of citric acid in solution B is 0.1-1 mmol / mL, preferably 0.25-0.4 mmol / L.
6. The method for preparing a cobalt-based MOF carbon absorbing material according to claim 3, characterized in that In step 3), the temperature of the hydrothermal reaction is 100-130° C., preferably 110-120° C., and the time of the hydrothermal reaction is 24-60 h, preferably 40-48 h.
7. The method for preparing a cobalt-based MOF carbon absorbing material according to claim 3, characterized in that In step 4), the inert gas is nitrogen, and the high temperature annealing operation is: heating to 600-800°C at a heating rate of 1°C / min-10°C / min, then keeping the temperature for 2-3 hours, and then cooling to room temperature at a rate of 1°C / min-10°C / min.
8. The method for preparing a cobalt-based MOF carbon absorbing material according to claim 7, characterized in that The heating rate is 4-5 ℃ / min, the holding temperature is 650-700 ℃, and the cooling rate is 2-3 ℃ / min.
9. A cobalt-based MOF carbon absorbing material prepared by the method according to any one of claims 1 to 8.
10. Use of the cobalt-based MOF carbon absorbing material as claimed in claim 9 in microwave absorption.
Citation Information
Patent Citations
Method for preparing MOFs (metal organic frameworks) material with function of adsorbing CO2 in biogas
CN103920464A
Preparation method and application of bimetallic MOFs loaded alumina spheres
CN112691644A
Cited By
Wave-absorbing material as well as preparation method and application thereof
CN121851729A