Preparation method and application of composite graphitized carbon carrier

The carbon carrier preparation method through wet mixing and shearing crushing treatment, combined with high oxygen atmosphere graphitization and puffing crushing treatment, solves the problems of unstable carbon support material structure and low catalyst utilization rate, and achieves high catalytic activity and durability. composite graphitized carbon carrier.

CN118723988AInactive Publication Date: 2024-10-01ZHEJIANG FENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410772783.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing carbon support materials are structurally unstable at high temperatures, and their pore structure results in low catalyst utilization and poor durability. It is also difficult for composite carbon-based materials to build a three-dimensional composite network structure, which affects catalytic performance and mechanical strength.

Method used

Through wet mixing of granular and linear carbon materials, shearing and crushing treatment, high oxygen atmosphere graphitization treatment, and puffing and crushing treatment, the preparation method of graphitized carbon carrier is optimized to build a three-dimensional composite network structure and improve the conductivity and mechanical strength. .

Benefits of technology

A composite graphitized carbon carrier with high specific surface area and stable three-dimensional composite network structure is achieved, which improves the catalytic activity and durability of the catalyst and ensures uniform dispersion and high utilization of precious metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723988A_ABST
    Figure CN118723988A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a composite graphitized carbon carrier. The preparation method comprises the following steps: (1) carrying out wet mixing on a granular carbon material and a linear carbon material, and shearing and crushing to obtain a mixed carbon-based material; (2) carrying out primary impurity removal treatment on the mixed carbon-based material by utilizing an acid solution, then washing to be neutral, and drying to obtain a pretreated mixed carbon-based material; (3) carrying out graphitization treatment on the pretreated mixed carbon-based material in a high-oxygen atmosphere to obtain a graphitized carbon material; and (4) carrying out secondary impurity removal treatment on the graphitized carbon material by using an acid solution, then washing the graphitized carbon material to be neutral, drying, cooling, and carrying out puffing and crushing treatment to obtain the composite graphitized carbon carrier. The two carbon materials in the composite graphitized carbon carrier prepared by the method are uniformly distributed, the granular carbon material can be embedded between the linear carbon materials to form a more stable three-dimensional composite network structure, and the catalytic activity and durability of the catalyst can be effectively improved by combining high graphitization and high specific surface area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalytic materials, and in particular to a preparation method and application of a composite graphitized carbon carrier. Background Art

[0002] Carbon materials have good acid and alkali resistance, stable structure at high temperature, can be prepared into different physical forms, and the metal phase is easy to reduce. They are widely used as catalyst carriers, especially for loading precious metals. For example, carbon black, a catalyst carrier material commonly used in fuel cells, has a large specific surface area, good conductivity, suitable pore structure and low cost, making it a commonly used carrier material. Compared with single platinum black, the use of carbon black to load platinum can improve catalytic activity, thanks to the uniform dispersion of metal platinum on the surface of carbon black. However, due to the presence of a large number of micropores in the pore structure of carbon black, the metal platinum deposited and in the micropores cannot play a catalytic role, reducing the utilization rate of platinum. In addition to the above-mentioned single graphitized carrier, the use of mixed carriers that have not been graphitized also has the problem of low catalyst utilization due to surface micropores, and the durability is also relatively poor.

[0003] Based on the problems existing in the above-mentioned carbon carriers, patent CN115566212A discloses a metal catalyst with graphitized composite carbon as a carrier and a preparation method thereof, wherein a composite carbon-based material obtained by mixing and graphitizing granular carbon material and linear carbon material is used as a catalyst carrier for loading platinum alloys. The three-dimensional composite network structure formed based on the granular carbon material and the linear carbon material increases the three-phase reaction zone and mechanical strength of the catalyst, thereby improving the utilization rate and durability of metal platinum. However, in the actual preparation process, since the granular carbon material and the linear carbon material have a large specific surface energy and are easy to agglomerate, the composite carbon-based material prepared by the method described in the above patent will show the phenomenon of separate agglomeration of granular carbon material and linear carbon material, and the granular carbon material is difficult to embed between the linear carbon materials, and it is impossible to effectively construct a three-dimensional composite network structure, which is not conducive to the increase in the specific surface area of ​​the composite carbon-based material and the increase in the three-phase reaction zone of the catalyst; in addition, since the composite carbon-based material is only partially graphitized after graphitization treatment, the interior of the material is not fully graphitized, which affects the conductivity and mechanical strength of the composite carbon-based material, and further affects the catalytic performance and durability of the catalyst using the composite carbon-based material as a catalyst carrier. Summary of the invention

[0004] To solve the above problems, the present invention provides a method for preparing a composite graphitized carbon carrier and an application thereof. By optimizing the mixing method, graphitization treatment atmosphere and post-treatment, a composite graphitized carbon carrier with a three-dimensional composite network structure, high graphitization, high mechanical strength and high specific surface area is obtained. The composite graphitized carbon carrier is used as a catalytic carrier to load platinum to prepare a catalyst, which can effectively improve the catalytic activity and durability of the catalyst.

[0005] Specifically, the following technical solutions are provided:

[0006] The first aspect of the present invention provides a method for preparing a composite graphitized carbon carrier, comprising the following steps:

[0007] (1) Wet mixing of granular carbon material and linear carbon material, and shear crushing to obtain a mixed carbon-based material;

[0008] (2) using an acid solution to perform a decontamination treatment on the mixed carbon-based material, then washing it with water until it is neutral, and drying it to obtain a pretreated mixed carbon-based material;

[0009] (3) graphitizing the pretreated mixed carbon-based material in a high oxygen atmosphere to obtain a graphitized carbon material; the oxygen content in the high oxygen atmosphere is 80%-90%;

[0010] (4) The graphitized carbon material is subjected to secondary decontamination treatment using an acid solution, and then washed with water until neutral, dried, cooled, and then subjected to expansion and crushing treatment to obtain the composite graphitized carbon carrier.

[0011] Furthermore, in step (1), the granular carbon material includes one or more of mesoporous carbon, carbon spheres, and amorphous carbon; and the linear carbon material includes carbon nanotubes and / or carbon fibers.

[0012] Furthermore, in step (1), the mass ratio of the granular carbon material to the linear carbon material is preferably 5-8:1-2, for example 5:1, 6:1, 7:1, 8:1, 8:2, etc., including but not limited to the mass ratios listed above. The granular particles are generally larger than the linear materials. The linear materials mainly play the role of building the frame, and the granular materials are used to fill the gaps in the frame. Too much linear material will cause the frame to be too dense, making it difficult for the granular material to fill the gaps.

[0013] Furthermore, in step (1), the solvent for wet mixing is preferably ethylene glycol, which has good stability and can slow down the rate of carbon material agglomeration during the wet mixing process; more preferably, the ratio of the total mass of the granular carbon material and the linear carbon material to the mass of the alcohol solvent is 2-5:1-3, for example 2:1, 3:1, 4:1, 5:1, 2:2, 3:2, 5:2, 2:3, 4:3, 5:3, etc., including but not limited to the ratios listed above.

[0014] Furthermore, in step (1), the shearing and crushing step is carried out in a high-speed crusher, and the rotation speed of the high-speed crusher is not less than 10000rpm. Since the surface energy of granular and linear carbon materials is too high, agglomeration is very likely to occur during the mixing process, and it is difficult to embed the granular carbon materials into the connecting pores between the linear carbon materials, and it is impossible to achieve uniform mixing of the two carbon materials and the construction of a three-dimensional composite network structure; the present invention is conducive to breaking up the agglomeration between granular materials and linear materials through the shearing action of the high-speed crusher, achieving uniform dispersion of the two carbon materials, and at the same time promoting the embedding of granular carbon materials between adjacent linear carbon materials, thereby facilitating the construction of a three-dimensional composite network structure.

[0015] Furthermore, in step (2), the acid solution is preferably a nitric acid solution with a mass concentration of 10%-15%, for example, a nitric acid solution with a concentration of 10%, 12%, 13%, 14% or 15%; the nitric acid solution is used to remove metal impurities in the mixed carbon-based material, including but not limited to iron.

[0016] Furthermore, in step (2), the temperature of the first de-impurity treatment is preferably 95-100° C., and the time is preferably 2-3 h.

[0017] Furthermore, in step (2), the drying is vacuum drying, and the drying temperature is preferably 190-220°C.

[0018] Furthermore, in step (3), the graphitization treatment is controlled to be carried out in a high oxygen atmosphere, for example, the graphitization treatment is carried out in an atmosphere with an oxygen content of 80%, 85% or 90%, so as to increase the change activity of the carbon material at high temperature and make the graphitization degree of the carbon material more complete. During the graphitization treatment process, if the oxygen content is too low, the carbon material will have problems of partial graphitization and incomplete graphitization, which will affect the conductivity and mechanical strength of the material; but if the oxygen content is too high, it is easy to explode. Therefore, under the premise of ensuring safety, the pretreated mixed carbon-based material can be fully graphitized, and the oxygen content in the graphitization treatment atmosphere is preferably controlled between 80% and 90%.

[0019] Further, in step (3), in the graphitization treatment step: first sinter at 1900℃-2200℃ for 3-5h, then heat to 2700℃-2900℃ and sinter for 3-5h; for example, first sinter at 2000℃ for 4 hours, then heat to 2800℃ and sinter for another 4 hours.

[0020] Furthermore, in step (4), the acid solution is preferably a sulfuric acid solution with a mass concentration of 5%-8%, for example, a sulfuric acid solution with a concentration of 5%, 6%, 7% or 8%, and the sulfuric acid solution is used to further remove metal impurities in the graphitized carbon material, such as copper and iron impurities.

[0021] Furthermore, in step (4), the temperature of the secondary de-impurity treatment is 95-100° C. and the time is 2-3 hours.

[0022] Furthermore, in step (4), the drying temperature is 200-250°C.

[0023] Furthermore, in step (4), after the temperature drops to below 60°C, an expansion and crushing treatment is performed; the expansion and crushing treatment is a dry expansion and crushing treatment performed in an expansion processing machine, and the expansion and crushing treatment time is 3-5h. After high-temperature graphitization treatment and secondary impurity removal treatment, some carbon carriers will agglomerate. Directly using them to load metals will result in low loading rates and large differences in the performance of the prepared catalyst. The present invention expands and crushes the dried composite graphitized carbon carrier to disperse the agglomerated carbon carriers to obtain a carbon carrier with uniform size and high specific surface area.

[0024] The second aspect of the present invention provides a composite graphitized carbon carrier prepared by the preparation method described in the first aspect.

[0025] Furthermore, the particle size of the composite graphitized carbon carrier is less than 5 nm.

[0026] The third aspect of the present invention provides an application of the composite graphitized carbon carrier described in the second aspect as a catalyst carrier.

[0027] Furthermore, the composite graphitized carrier is used as a catalyst carrier to load platinum.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. The present invention provides a method for preparing a composite graphitized carbon carrier, wherein a granular carbon material and a linear carbon material are mixed by wet mixing and shear crushing, so that the two carbon materials can be fully mixed and uniform and the granular carbon material can be effectively embedded between adjacent linear carbon materials, thereby effectively constructing a three-dimensional composite network structure; then, a graphitization treatment is performed in a high oxygen atmosphere, so that the mixed carbon-based material can be fully graphitized to obtain a composite graphitized carbon carrier with high conductivity and high mechanical strength; finally, the graphitized carbon carrier is expanded and crushed to obtain a composite graphitized carbon carrier of uniform size and dispersion. The composite graphitized carbon carrier prepared by the above preparation method has a stable three-dimensional composite network structure, and has good conductivity, high mechanical strength and high specific surface area.

[0030] 2. The above-mentioned composite graphitized carbon carrier is used to load precious metal catalysts. The composite graphitized carbon carrier with high specific surface area is conducive to the uniform dispersion of precious metals and improves the utilization rate of precious metals. The three-dimensional composite network structure constructed by uniformly distributed granular carbon materials and linear carbon materials enhances the contact between the active substance and the current collector and the proton membrane, increases the three-phase reaction active area of ​​the catalyst, and the composite graphitized carbon carrier has good electrical conductivity, which is conducive to improving the catalytic activity. In addition, the highly graphitized carbon carrier has high mechanical strength, which can effectively improve the durability of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a comparison chart of the CV performance of the composite graphitized carbon support catalyst prepared in Examples 1 and 2 and Comparative Example 1;

[0032] Figure 2 This is a comparison chart of the LSV performance of the composite graphitized carbon carrier catalyst prepared in Example 1 and Comparative Example 1;

[0033] Figure 3 This is a performance test comparison chart of film-forming electrodes prepared by different composite graphitized carbon carrier catalysts;

[0034] Figure 4 The durability test results of the catalyst in Example 1 are shown in FIG. DETAILED DESCRIPTION

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0036] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0037] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0038] Example 1

[0039] This embodiment relates to the preparation of a composite graphitized carbon carrier and a fuel cell catalyst, and the specific operations are as follows:

[0040] Preparation of composite graphitized carbon carrier:

[0041] (1) A granular carbon material (carbon black EC600jd) and a linear carbon material (carbon nanotube XFM13) were mixed at a mass ratio of 5:1 to obtain a carbon-based material; then ethylene glycol (the mass ratio of the carbon-based material to ethylene glycol was 2:1) was added and stirred thoroughly, and a high-speed shearing machine was used for shearing at a shearing speed of 10000 r / h and a shearing time of 1 h to obtain a mixed carbon-based material;

[0042] (2) adding a 10% dilute nitric acid solution to the mixed carbon-based material, heating the temperature to 95° C., stirring for 2 hours, then washing the mixed carbon-based material with ultrapure water until neutral, and drying in an oven at 180° C. to obtain the pretreated mixed carbon-based material for standby use;

[0043] (3) placing the pretreated mixed carbon-based material in a high-temperature furnace, introducing oxygen until the oxygen content reaches 80%, and performing graphitization treatment. After sintering at 2000° C. for 4 hours, the temperature is increased to 2800° C. and sintered for another 4 hours to obtain a graphitized carbon material;

[0044] (4) Add 6% sulfuric acid solution to the graphitized carbon material, stir at 95° C. for 2 hours, then wash the mixed carbon-based material with ultrapure water until it is neutral, dry it in an oven at 180° C., wait for the temperature to drop to 60° C., take it out and place it in an expander for dry expansion and crushing treatment to obtain a composite graphitized carbon carrier with a particle size of 3-5 nm.

[0045] Preparation of catalyst:

[0046] (1) adding the composite graphitized carbon support prepared in this example to a mixed solvent of ethylene glycol and water (the volume ratio of ethylene glycol to water is 1.5:3), ultrasonically dispersing, and then adding the dispersion to a synthesis chamber for stirring;

[0047] (2) dissolving Cl6H2Pt in an organic solvent to obtain a metal salt precursor solution; wherein the content of the metal salt precursor Cl6H2Pt in the metal salt precursor solution is 10 g / L;

[0048] (3) adding the metal precursor solution into the synthesis chamber, adding sodium hydroxide to adjust the pH to 12, and conducting an anaerobic reaction under nitrogen for 4 hours to obtain a catalyst precursor;

[0049] (4) The obtained catalyst precursor is washed and filtered to remove alcohol substances, and then vacuum dried and expanded to obtain a catalyst Pt / C-HT-1 with a graphitized carbon-based material as a carrier.

[0050] Example 2

[0051] This embodiment relates to the preparation of a composite graphitized carbon carrier and a fuel cell catalyst, and the specific operations are as follows:

[0052] Preparation of composite graphitized carbon carrier:

[0053] (1) A granular carbon material (carbon black XC-72R) and a linear carbon material (carbon nanotube CNT-102-107) were mixed at a mass ratio of 5:1 to obtain a carbon-based material; then ethylene glycol (the mass ratio of the carbon-based material to the ethylene glycol was 2:1) was added and stirred thoroughly, and a high-speed shearing machine was used for shearing at a shearing speed of 10000 r / h and a shearing time of 1 h to obtain a mixed carbon-based material;

[0054] (2) adding a 10% dilute nitric acid solution to the mixed carbon-based material, heating the temperature to 95° C., stirring for 2 hours, then washing the mixed carbon-based material with ultrapure water until neutral, and drying in an oven at 180° C. to obtain the pretreated mixed carbon-based material for standby use;

[0055] (3) placing the pretreated mixed carbon-based material in a high-temperature furnace, introducing oxygen until the oxygen content reaches 80%, and performing graphitization treatment. After sintering at 2000° C. for 4 hours, the temperature is increased to 2800° C. and sintered for another 4 hours to obtain a graphitized carbon material;

[0056] (4) Add 6% sulfuric acid solution to the graphitized carbon material, stir at 95° C. for 2 hours, then wash the mixed carbon-based material with ultrapure water until it is neutral, dry it in an oven at 180° C., wait for the temperature to drop to 60° C., take it out and place it in an expander for dry expansion and crushing treatment to obtain a composite graphitized carbon carrier with a particle size of 3-5 nm.

[0057] Preparation of catalyst:

[0058] (5) adding the composite graphitized carbon support prepared in this example to a mixed solvent of ethylene glycol and water (the volume ratio of ethylene glycol to water is 1.5:3), ultrasonically dispersing, and then adding the dispersion to a synthesis chamber for stirring;

[0059] (6) dissolving Cl6H2Pt in an organic solvent to obtain a metal salt precursor solution; wherein the content of the metal salt precursor Cl6H2Pt in the metal salt precursor solution is 10 g / L;

[0060] (7) adding the metal precursor solution into the synthesis chamber, adding sodium hydroxide to adjust the pH to 12, and conducting an anaerobic reaction under nitrogen for 4 hours to obtain a catalyst precursor;

[0061] (8) The obtained catalyst precursor is washed and filtered to remove alcohol substances, and then vacuum dried and expanded to obtain a catalyst Pt / C-HT-2 with a graphitized carbon-based material as a carrier.

[0062] Comparative Example

[0063] This comparative example relates to the preparation of a composite graphitized carbon carrier and a fuel cell catalyst, wherein the composite graphitized carbon carrier is prepared by the method described in CN115566212A, and the specific operation is as follows:

[0064] Preparation of composite graphitized carbon carrier:

[0065] (1) granular carbon (mesoporous carbon CA) and linear carbon material (carbon nanotube XFM13) were mixed in a horizontal ball mill at a mass ratio of 10:3 to obtain a carbon-based material, added to a 5% dilute nitric acid solution, heated at 95° C., stirred for 2 hours, washed the mixed carbon-based material until the pH was neutral, and dried in an oven at 180° C. for later use;

[0066] (2) The obtained carbon-based material was graphitized in an air atmosphere, placed in a high-temperature furnace and sintered at 1800°C for 4 hours, then the temperature was raised to 2600°C and sintered for 4 hours, cooled and taken out, and the carbon-based material was subjected to a secondary decontamination treatment by adding 5% dilute sulfuric acid and stirring at 90°C for 2 hours, washing the carbon-based material until the pH was neutral, and drying in an oven at 180°C for use.

[0067] Preparation of catalyst:

[0068] (1) adding the composite graphitized carbon support prepared in this comparative example to a mixed solvent of ethylene glycol and water (the mass ratio of the carbon support, ethylene glycol and water is 0.5:1.5:3), ultrasonically dispersing, and then adding the dispersion to a synthesis chamber and stirring;

[0069] (2) dissolving Cl6H2Pt in an organic solvent to obtain a metal salt precursor solution; wherein the content of the metal salt precursor Cl6H2Pt in the metal salt precursor solution is 10 g / L;

[0070] (3) adding the metal precursor solution into the synthesis chamber, adding sodium hydroxide to adjust the pH to 12, and conducting an anaerobic reaction under nitrogen for 4 hours to obtain a catalyst precursor;

[0071] (4) washing and filtering the obtained catalyst precursor to remove alcohol substances, vacuum drying and expansion to obtain a catalyst Pt / C with a graphitized carbon-based material as a carrier. A +XFM13.

[0072] Performance Testing

[0073] The catalysts prepared in the above examples and comparative examples were sampled and tested according to national standards, as follows:

[0074] The CV performance of the catalysts prepared in Examples 1 and 2 and the comparative example was tested. The test results are as follows: Figure 1 As shown, the CV performance of the catalysts prepared in Examples 1 and 2 is significantly better than that of the comparative example;

[0075] The LSV performance of the catalysts prepared in Example 1 and the comparative example was tested. Figure 2 It can be seen that the LSV performance of the catalyst prepared in Example 1 is better than that of the comparative catalyst Pt / C A +XFM13;

[0076] The catalysts prepared in the examples and comparative examples were used to prepare membrane electrodes (only the catalyst types were different, and the other materials and operations were the same), and the I / V curves of different membrane electrodes were tested. The test results are shown in FIG. Figure 3 As shown, the membrane electrode containing the catalyst prepared in Examples 1 and 2 has a higher current density at low voltage, indicating that the electrochemical reaction rate at low voltage is faster and has a better catalytic effect. Figure 4 It can be seen that the one prepared in Example 1 has good durability.

[0077] In summary, the present invention optimizes the mixing method of the two carbon materials, the graphitization treatment atmosphere and the post-treatment to prepare a composite graphitized carbon carrier for loading platinum, which has better catalytic performance and aging resistance.

[0078] The above-mentioned embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by technicians in the technical field on the basis of the present invention are all within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for preparing a composite graphitized carbon carrier, characterized in that: The following steps are involved: (1) Wet mixing of granular carbon material and linear carbon material, and shear crushing to obtain a mixed carbon-based material; (2) using an acid solution to perform a decontamination treatment on the mixed carbon-based material, then washing it with water until it is neutral, and drying it to obtain a pretreated mixed carbon-based material; (3) graphitizing the pretreated mixed carbon-based material in a high oxygen atmosphere to obtain a graphitized carbon material; the volume content of oxygen in the high oxygen atmosphere is 80%-90%; (4) The graphitized carbon material is subjected to secondary decontamination treatment using an acid solution, and then washed with water until neutral, dried, cooled, and then subjected to expansion and crushing treatment to obtain the composite graphitized carbon carrier.

2. The preparation method according to claim 1, characterized in that: In step (1), the granular carbon material includes one or more of mesoporous carbon, carbon spheres, and amorphous carbon; the linear carbon material includes carbon nanotubes and / or carbon fibers; The mass ratio of the granular carbon material to the linear carbon material is 5-8:1-2.

3. The preparation method according to claim 1, characterized in that: In step (1), the solvent for wet mixing is an alcohol solvent; Preferably, the ratio of the total mass of the granular carbon material and the linear carbon material to the mass of the alcohol solvent is 2-5:1-3; Preferably, the alcohol solvent is ethylene glycol; Preferably, the shearing and crushing step is carried out in a high-speed crusher, and the rotation speed of the high-speed crusher is not less than 10000 rpm.

4. The preparation method according to claim 1, characterized in that: In step (2), the acid solution is a nitric acid solution, and preferably, the mass concentration of the nitric acid solution is 10%-15%; Preferably, the temperature of the first impurity removal treatment is 95-100°C and the time is 2-3h; Preferably, the drying is vacuum drying at a temperature of 190-220°C.

5. The preparation method according to claim 1, characterized in that: In step (3), in the graphitization treatment step: first sinter at 1900°C-2200°C for 3-5h, then heat to 2700°C-2900°C and sinter for 3-5h.

6. The preparation method according to claim 1, characterized in that: In step (4), the acid solution is a sulfuric acid solution, and preferably, the mass concentration of the sulfuric acid solution is 5%-8%; The temperature of the secondary impurity removal treatment is 95-100°C and the time is 2-3h; The drying temperature is 200-250°C.

7. The preparation method according to claim 1, characterized in that: In step (4), after the temperature is lowered to below 60° C., expansion and crushing treatment is performed; The puffing and crushing process is a dry puffing and crushing process carried out in a puffing processor, and the puffing and crushing process takes 3-5 hours.

8. A composite graphitized carbon carrier prepared by the preparation method according to any one of claims 1 to 7.

9. The composite graphitized carbon carrier according to claim 8, characterized in that The primary particle size of the composite graphitized carbon carrier is less than 5 nm.

10. Use of the composite graphitized carbon carrier according to claim 8 or 9 as a catalyst carrier.

Citation Information

Patent Citations

  • Metal catalyst taking graphitized composite carbon as carrier as well as preparation method and application of metal catalyst

    CN115566212A

  • Process for mass-producing silicon nanowires and silicon nanowire-graphene hybrid particulates