Preparation method of tabular crystal tungsten carbide powder and tabular crystal tungsten carbide powder

By calcining tungsten trioxide, organic carbon source, anhydrous glucose, and sodium chloride under a high-temperature inert atmosphere, the problem of difficulty in preparing plate-shaped crystalline tungsten carbide powder in the existing technology is solved, and high strength, high hardness, and The preparation of plate-shaped crystalline tungsten carbide powder with high toughness and simple process is suitable for industrial production.

CN118723993APending Publication Date: 2024-10-01SICHUAN UNIVERSITY OF SCIENCE AND ENGINEERING

Patent Information

Application Number
CN202410785973.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to prepare plate-like crystalline tungsten carbide powder with high strength, high hardness and high toughness using the existing technology. In the traditional method, the WC grains have a truncated pyramidal prism structure, and the introduced molding agent will reduce the toughness of the cemented carbide.

Method used

Tungsten trioxide, organic carbon source, anhydrous glucose, and sodium chloride are used as mixed raw materials. They are mixed by ball milling and then calcined in a high-temperature inert atmosphere. They are cleaned and dried to directly obtain plate-shaped crystalline tungsten carbide powder. No addition is required in the entire process. Shaping agents and crystal growth additives.

Benefits of technology

The particle size of the plate-like crystal structure in tungsten carbide is adjustable, the degree of plate-like formation is high, the process is simple, the cost is low, it is suitable for industrial large-scale production, and the production process is safe and reliable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723993A_ABST
    Figure CN118723993A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of tabular crystal tungsten carbide powder and the tabular crystal tungsten carbide powder.The method comprises the steps that tungsten trioxide, an organic carbon source, glucose and sodium chloride are subjected to ball-milling mixing, and after mixed materials and ball-milling balls are screened and separated, mixed powder A is obtained; putting the mixed powder A into a high-purity graphite crucible, putting the high-purity graphite crucible into a calcining furnace, carrying out high-temperature calcination in an inert gas atmosphere, carrying out heat preservation, and cooling to room temperature to obtain a calcined product B; cleaning and filtering the calcined product B to obtain a carbonized substance C; and the carbonized substance C is dried, and the tabular crystal tungsten carbide powder is obtained. According to the method, the tungsten trioxide, the organic carbon source, the anhydrous dextrose and the sodium chloride are directly ball-milled and mixed, then the ball-milled and mixed powder is directly subjected to high-temperature calcination, and then the calcined product is filtered and dried to obtain the tabular crystal tungsten carbide powder, so that the technological process is simple, a crystal growth additive does not need to be added, the technological conditions are simple and easy to control, and the method is suitable for industrial production. The method is suitable for industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tungsten carbide material processing, and in particular, relates to a method for preparing plate-like crystal tungsten carbide powder and the plate-like crystal tungsten carbide powder. Background Art

[0002] Tungsten carbide (WC) particles are anisotropic crystals, and the hardness of the (0001) basal plane is 2100HV, which is about twice that of the (10-10) facet (1080HV). In addition, the strength of the (0001) basal plane reaches 12.5GPa, which is also greater than the 7.2GPa of the (10-10) facet. Therefore, when the WC grains in the WC-Co cemented carbide are plate-like structures, the hardness and strength of the cemented carbide can be improved. At the same time, the plate-like WC crystals are conducive to the plate-like and bridging of cracks, thereby improving the toughness of the cemented carbide. Therefore, compared with traditional cemented carbide, plate-like crystal cemented carbide has the characteristics of high strength, high hardness and high toughness, thus becoming a development trend of cemented carbide materials.

[0003] At present, the main preparation method of tungsten carbide (WC) powder is to mix tungsten powder (W) and carbon black (C), and then carbonize them into WC powder at high temperature (1300-2000℃). However, this tungsten carbide powder is spherical particles, and the cemented carbide sintered by this WC body is a traditional cemented carbide, whose WC grains are truncated cone triangular prisms, and it is impossible to prepare plate-like tungsten carbide powder. In addition, WO3 and carbon black are mixed into a slurry, and crystal growth agents such as Cr3C2 and TiC are added, followed by spray drying to obtain a mixture, and finally calcined at a high temperature of 1500-1700℃ to prepare a plate-like WC powder. However, the introduction of Cr3C2 and TiC will significantly reduce the toughness of the cemented carbide. Summary of the invention

[0004] The purpose of the embodiment of the present invention is to provide a method for preparing plate-like tungsten carbide powder with adjustable WC particle size, simple and controllable reaction process and simple preparation process flow. Tungsten trioxide (WO3), organic carbon source, anhydrous glucose and sodium chloride are used as mixed raw materials, and plate-like tungsten carbide powder can be obtained by direct calcination.

[0005] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing plate-like tungsten carbide powder, comprising the following steps:

[0006] Step S01: ball-milling tungsten trioxide, an organic carbon source, glucose and sodium chloride, and sieving the mixture and the grinding balls to obtain a mixed powder A;

[0007] Step S02: putting the mixed powder A into a high-purity graphite crucible, and placing it in a calcining furnace, calcining it at high temperature under an inert gas atmosphere, keeping the temperature, and cooling it to room temperature to obtain a calcined product B;

[0008] Step S03: washing and filtering the calcined product B to obtain a carbonized material C;

[0009] Step S04: drying the carbide material C to obtain plate-like tungsten carbide powder;

[0010] Wherein, in the step S01, the mass ratio of the tungsten trioxide, the organic carbon source, the glucose and the sodium chloride is 1:(1-1.5):(0-0.05):(0.25-1).

[0011] Optionally, in step S01, the organic carbon source is at least one of dicyandiamide and melamine.

[0012] Optionally, in step S01, the ball-to-material ratio of the ball milling mixing treatment is (1-3):1, and the ball milling time is 6-12 hours.

[0013] Optionally, in step S02, the high temperature calcination temperature is 1180-1200°C, and the holding time is 2-6 hours.

[0014] Optionally, the high-temperature calcination is divided into two stages. In the first stage, the temperature is increased to 700° C. at 2° C. / min and kept at this temperature for 0.5 h. In the second stage, the temperature is increased to 1180-1200° C. at 2° C. / min and kept at this temperature for 2-6 h.

[0015] Optionally, in step S03, the calcined product B is filtered 3 to 5 times with deionized water.

[0016] Optionally, in step S04, the temperature of the drying process is 60 to 100° C., and the time of the drying process is 2 to 6 hours.

[0017] Optionally, in step S02, the inert gas is argon, and the flow rate of the argon gas introduced into the calcining furnace is controlled to be 100-300 ml / min.

[0018] Optionally, in the step S01, a 40-80 mesh screen is used to screen the ball material mixture after ball milling.

[0019] Another object of an embodiment of the present invention is to provide a method for preparing plate-like tungsten carbide powder by using the above-mentioned method for preparing plate-like tungsten carbide powder.

[0020] To achieve the above object, the technical solution adopted by the present invention is: to provide a plate-like tungsten carbide powder, wherein the plate-like tungsten carbide powder is prepared by the above-mentioned method for preparing the plate-like tungsten carbide powder.

[0021] Compared with the prior art, the one or more technical solutions in the embodiments of the present invention have at least one of the following beneficial effects:

[0022] The method for preparing plate-like tungsten carbide powder in the embodiment of the present invention directly ball-mills tungsten trioxide, organic carbon source, anhydrous glucose and sodium chloride, and then directly calcines the mixed powder after ball milling at high temperature, and then washes, filters and dries the calcined product to obtain plate-like tungsten carbide powder. The entire preparation process does not require the addition of molding agents and crystal growth additives. The process conditions are simple and easy to control, the production cost is low, and it is suitable for industrial large-scale production. In addition, the plate-like tungsten carbide powder prepared by the method for preparing plate-like tungsten carbide powder in the embodiment of the present invention has the characteristics of adjustable plate-like crystal structure particle size in tungsten carbide, high plate-like degree and simple process flow, and the entire production process is safe and reliable. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0024] Figure 1 is the XRD pattern of WC powder in Example 1 of the present invention;

[0025] Figure 2 This is a SEM image of the WC powder in Example 1 of the present invention;

[0026] Figure 3 is the XRD pattern of WC powder in Example 2 of the present invention;

[0027] Figure 4 This is a SEM image of WC powder in Example 2 of the present invention;

[0028] Figure 5 is the XRD pattern of WC powder in Example 3 of the present invention;

[0029] Figure 6 This is a SEM image of WC powder in Example 3 of the present invention;

[0030] Figure 7 is the XRD pattern of WC powder in Example 4 of the present invention;

[0031] Figure 8 This is a SEM image of WC powder in Example 4 of the present invention;

[0032] Fig. 9 is the XRD pattern of WC powder in Example 5 of the present invention;

[0033] Fig.10 This is the SEM image of the WC powder in Example 5 of the present invention. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0035] The embodiment of the present invention provides a method for preparing plate-like tungsten carbide powder, comprising the following steps:

[0036] Step S01: ball-milling tungsten trioxide, an organic carbon source, glucose and sodium chloride, and sieving and separating the mixed material and the ball milling balls to obtain a mixed powder A;

[0037] Step S02: putting the mixed powder A into a high-purity graphite crucible, and placing it in a calcining furnace, calcining it at high temperature under an inert gas atmosphere, keeping the temperature, and cooling it to room temperature to obtain a calcined product B;

[0038] Step S03: washing and filtering the calcined product B to obtain a carbonized material C;

[0039] Step S04: Dry the carbide material C to obtain plate-like tungsten carbide powder.

[0040] The preparation method and technical scheme of the present invention are further explained in detail below.

[0041] In step S01, the organic carbon source refers to a material that can provide a source of carbon elements for tungsten carbide. In the process of the organic carbon source reacting to generate tungsten carbide, the carbon element provided by the organic carbon source reacts chemically with the tungsten element in tungsten trioxide to generate a tungsten carbide compound. Preferably, the organic carbon source is at least one of dicyandiamide and melamine. Among them, the mass ratio of tungsten trioxide, organic carbon source, glucose and sodium chloride is 1: (1-1.5): (0-0.05): (0.25-1). The mass ratio of tungsten trioxide, organic carbon source, glucose and sodium chloride can control the growth of tungsten carbide toward a plate-like crystal structure during high-temperature calcination, which is beneficial to improve the plate-like degree of tungsten carbide. When the tungsten trioxide content is too low, the carbon content in the organic carbon source exceeds the reaction ratio of reduction carbonization, resulting in excessive free carbon, which is not conducive to subsequent use; when the tungsten trioxide content is too high, the total carbon is less than the theoretical value after reduction carbonization, that is, the total carbon is too small, and decarburized W2C and W phases will be formed, which will cause carbon deficiency to the subsequent use of plate-like tungsten carbide to produce alloys and other applications; when the organic carbon source content is too low, decarburized phases such as W2C and W phases will be formed, affecting the growth of plate-like crystal structure; when the organic carbon source content is too high, the free carbon content of the product plate-like tungsten carbide is high, which will cause carburization to the subsequent use of plate-like tungsten carbide to produce alloys and other applications. In addition, the addition of glucose can increase the yield of plate-like tungsten carbide powder. However, excessive addition of glucose will not only not increase the yield of plate-like tungsten carbide powder, but also inhibit the formation of plate-like crystal structure, thereby reducing the yield of plate-like tungsten carbide powder.

[0042] In step S01, a ball mill is used to mix tungsten trioxide, an organic carbon source, glucose, and sodium chloride by ball milling. The ball mill can be, but is not limited to, a stirring ball mill, a drum ball mill, or a vibrating ball mill. The ball milling balls used for the grinding balls are made of stainless steel or cemented carbide, and the ball milling jars are made of stainless steel, polyethylene, or polytetrafluoroethylene. The ball-to-material ratio of the ball milling mixing treatment is (1-3):1, and the ball milling time is 6-12 hours. When the ball-to-material ratio is too large, the grinding impact intensity is uneven, resulting in a relatively wide distribution of the grinding particle size of each component, causing irregular growth of tungsten carbide; and if the ball-to-material ratio is too small, the grinding efficiency is low and a longer grinding time is required. If the ball milling time is too short, the brittle tungsten oxide cannot be fully ground and crushed, and the dispersion is uneven; and if the ball milling time is too long, the energy consumption will increase. Therefore, by using the ball-to-material ratio and ball milling time of the present application, the brittle tungsten trioxide can be quickly ground and crushed to achieve a uniform dispersion effect, while reducing the impurity content and saving energy consumption. When the grinding ball content is too low, the ball milling particle size and uniformity of tungsten trioxide, organic carbon source, glucose and sodium chloride are poor; when the grinding ball content is too high, the ball milling uniformity is good, but the impurity content increases, affecting the normal growth of plate-like tungsten carbide.

[0043] In step S01, since tungsten trioxide has low hardness and brittle texture, high-energy ball milling is not required. Conventional ball milling can evenly disperse and mix tungsten trioxide, organic carbon source, glucose and sodium chloride. A 40-80 mesh sieve is used to sieve the ball material mixture after ball milling to obtain a mixed powder.

[0044] In step S02, the temperature of high temperature calcination is 1180-1200°C, and the holding time is 2-6 hours. The high temperature calcination is divided into two stages. The first stage is to heat up to 700°C at 2°C / min and keep warm for 0.5 hours; the second stage is to heat up to 1180-1200°C at 2°C / min and keep warm for 2-6 hours. More preferably, before the calcination treatment, the tungsten trioxide, organic carbon source, glucose and sodium chloride are ball-milled and mixed to make the calcination faster.

[0045] In step S02, the inert gas is argon, and the flow rate of argon into the calcining furnace is controlled to be 100-300 ml / min. During the calcining process, the gas used to form an inert atmosphere is argon or nitrogen, and of course it can also be other gases that do not participate in the reaction of tungsten carbide products at high temperatures. In an inert atmosphere such as argon, the mixed powder is carbonized at high temperature to obtain plate-like tungsten carbide powder.

[0046] In step S03, the calcined product B is filtered 3 to 5 times with deionized water. In step S04, the drying temperature is 60 to 100° C., and the drying time is 2 to 6 hours. During the drying process, in order to avoid oxidation reaction and affect the final product, the product is dried in a vacuum environment at a temperature of 60 to 100° C. to accelerate the volatilization of water.

[0047] The method for preparing plate-like tungsten carbide powder provided by the present invention comprises directly ball-milling tungsten trioxide, an organic carbon source, anhydrous glucose and sodium chloride, and then directly calcining the mixed powder after ball-milling at high temperature, and then washing, filtering and drying the calcined product to obtain plate-like tungsten carbide powder. The whole preparation process does not require the addition of a molding agent and a crystal growth additive, and the process conditions are simple and easy to control, the production cost is low, and it is suitable for industrial large-scale production. In addition, the method for preparing plate-like tungsten carbide powder in the embodiment of the present invention has the characteristics of adjustable plate-like crystal structure particle size in tungsten carbide, high plate-like degree and simple process flow, and the whole production process is safe and reliable.

[0048] The present invention also provides a plate-like tungsten carbide powder prepared by the above-mentioned plate-like tungsten carbide powder preparation method, which has the characteristic of high plate-like degree in the tungsten carbide.

[0049] In order to more effectively illustrate the technical solution of the present invention, the technical solution of the present invention is described below through specific embodiments.

[0050] Example 1

[0051] (1) Weigh 50 g of tungsten trioxide, 50 g of melamine, 25 g of sodium chloride and 200 g of carbide grinding balls, put the above raw materials and grinding balls into a ball mill, and ball mill them on a drum ball mill for 10 h. Then, sieve with a 40-mesh screen to separate the mixed material and the grinding balls to obtain mixed powder A1.

[0052] (2) After the mixed powder A1 is loaded into a high-purity graphite crucible, it is placed in a calcining furnace and argon gas is introduced at a flow rate of 200 ml / min; in the first stage, the temperature is increased to 700°C at 2°C / min and kept at this temperature for 0.5 h; in the second stage, the temperature is increased to 1190°C at 2°C / min and kept at this temperature for 4 h. After the calcination is completed, it is cooled to room temperature in the furnace and the calcined product B1 is taken out.

[0053] (3) The calcined product B1 was washed with deionized water and filtered four times to obtain a carbonized material C1.

[0054] (4) The carbide material C1 is then placed in a drying oven and dried at 60° C. for 4 hours to obtain plate-like tungsten carbide powder.

[0055] The tungsten carbide powder in Example 1 was subjected to XRD analysis, and the results were as follows: Figure 1 As shown in Figure 1, the XRD pattern is consistent with the WC phase (JCPDS: 72-0097). SEM analysis of tungsten carbide powder shows the following results: Figure 2 As shown, the tungsten carbide particles are micron plate-like structures, and the average particle size of the plate-like crystal structure of the tungsten carbide particles is 3.9 μm.

[0056] Example 2

[0057] (1) Weigh 50 g of tungsten trioxide, 50 g of melamine, 25 g of sodium chloride and 300 g of carbide grinding balls, put the above raw materials and grinding balls into a ball mill, and ball mill them on a drum ball mill for 6 h. Then, sieve with a 60-mesh screen to separate the mixed material and the grinding balls to obtain mixed powder A2.

[0058] (2) After the mixed powder A2 is loaded into a high-purity graphite crucible, it is placed in a calcining furnace and argon gas is introduced at a flow rate of 100 ml / min; in the first stage, the temperature is increased to 700°C at 2°C / min and kept at this temperature for 0.5 h; in the second stage, the temperature is increased to 1180°C at 2°C / min and kept at this temperature for 2 h. After the calcination is completed, it is cooled to room temperature with the furnace and the calcined product B2 is taken out.

[0059] (3) The calcined product B2 was washed with deionized water and filtered three times to obtain a carbonized material C2.

[0060] (4) The carbide material C2 is placed in a drying oven and dried at 80°C for 2 hours to obtain plate-like tungsten carbide powder.

[0061] The tungsten carbide powder in Example 2 was subjected to X-ray powder diffraction (XRD) and scanning electron microscope (SEM) analysis, and the results were as follows: Figure 3 , Figure 4 As shown, the XRD spectrum is consistent with the WC phase (JCPDS: 72-0097). The tungsten carbide particles also have a micron plate structure, but the plate crystal structure size of the tungsten carbide particles is slightly reduced compared with Example 1, and the average particle size of the plate crystal structure of the tungsten carbide particles is 3.2 μm.

[0062] Example 3

[0063] (1) Weigh 50 g of tungsten trioxide, 50 g of dicyandiamide, 25 g of sodium chloride and 250 g of carbide grinding balls, put the above raw materials and grinding balls into a ball mill, and ball mill them on a drum ball mill for 12 h. Then, sieve with an 80-mesh screen to separate the mixed material and the grinding balls to obtain a mixed powder A3.

[0064] (2) After the mixed powder A3 is loaded into a high-purity graphite crucible, it is placed in a calcining furnace and argon gas is introduced at a flow rate of 300 ml / min; in the first stage, the temperature is increased to 700°C at 2°C / min and kept at this temperature for 0.5 h; in the second stage, the temperature is increased to 1200°C at 2°C / min and kept at this temperature for 6 h. After the calcination is completed, it is cooled to room temperature with the furnace and the calcined product B3 is taken out.

[0065] (3) The calcined product B3 was washed with deionized water and filtered three times to obtain a carbonized material C3.

[0066] (4) The carbide material C3 is then placed in a drying oven and dried at 100° C. for 6 hours to obtain plate-like tungsten carbide powder.

[0067] The tungsten carbide powder in Example 3 was subjected to X-ray powder diffraction (XRD) and scanning electron microscope (SEM) analysis, and the results were as follows: Figure 5 , Figure 6 As shown, the XRD spectrum is consistent with the WC phase (JCPDS: 72-0097). The tungsten carbide particles also have a micron plate structure, but the plate crystal structure size of the tungsten carbide particles is smaller than that of Example 1 and Example 2, and the average particle size of the plate crystal structure of the tungsten carbide particles is 1.2 μm.

[0068] Example 4

[0069] (1) Weigh 50 g of tungsten trioxide, 50 g of dicyandiamide, 50 g of sodium chloride, 1 g of anhydrous glucose and 200 g of carbide grinding balls, put the above raw materials and grinding balls into a ball mill, and ball mill them on a drum ball mill for 12 h. Then, sieve with a 40-mesh screen to separate the mixed material and the grinding balls to obtain a mixed powder A4.

[0070] (2) After the mixed powder A3 is loaded into a high-purity graphite crucible, it is placed in a calcining furnace and argon gas is introduced at a flow rate of 300 ml / min; in the first stage, the temperature is increased to 700°C at 2°C / min and kept at this temperature for 0.5 h; in the second stage, the temperature is increased to 1200°C at 2°C / min and kept at this temperature for 2 h. After the calcination is completed, it is cooled to room temperature with the furnace and the calcined product B4 is taken out.

[0071] (3) The calcined product B4 was washed with deionized water and filtered four times to obtain a carbonized material C4.

[0072] (4) The carbide material C4 is placed in a drying oven and dried at 90°C for 2 hours to obtain plate-like tungsten carbide powder.

[0073] The tungsten carbide powder in Example 4 was subjected to X-ray powder diffraction (XRD) and scanning electron microscope (SEM) analysis, and the results were as follows: Figure 7 , Figure 8 As shown, the XRD spectrum is consistent with the WC phase (JCPDS: 72-0097). The tungsten carbide particles are also micron plate-like structures, but the plate-like crystal structure size of the tungsten carbide particles is smaller than that of Example 1 and Example 2, but the plate-like degree and particle size of the plate-like crystal structure of the tungsten carbide particles are reduced, and the average particle size of the plate-like crystal structure is 1.0 μm.

[0074] Example 5

[0075] (1) Weigh 50 g of tungsten trioxide, 50 g of dicyandiamide, 50 g of sodium chloride, and 150 g of carbide grinding balls, put the above raw materials and grinding balls into a ball mill, and ball mill them on a drum ball mill for 12 h. Then, sieve with a 40-mesh screen to separate the mixed material and the grinding balls to obtain a mixed powder A5.

[0076] (2) After the mixed powder A5 is loaded into a high-purity graphite crucible, it is placed in a calcining furnace and argon gas is introduced at a flow rate of 200 ml / min; in the first stage, the temperature is increased to 700°C at 2°C / min and kept at this temperature for 0.5 h; in the second stage, the temperature is increased to 1200°C at 2°C / min and kept at this temperature for 6 h. After the calcination is completed, it is cooled to room temperature with the furnace and the calcined product B5 is taken out.

[0077] (3) The calcined product B5 was washed with deionized water and filtered five times to obtain a carbonized material C5.

[0078] (4) The carbide material C5 is placed in a drying oven and dried at 100° C. for 2 hours to obtain plate-like tungsten carbide powder.

[0079] The tungsten carbide powder in Example 5 was subjected to X-ray powder diffraction (XRD), and the results were as follows: Fig. 9As shown in FIG. 1 , the XRD pattern is consistent with the WC phase (JCPDS: 72-0097). The tungsten carbide powder in Example 5 was subjected to scanning electron microscopy (SEM) analysis, and the results are as follows: Fig.10 As shown, the tungsten carbide particles are micron plate-like structures, and the average particle size of the plate-like crystal structure of the tungsten carbide particles is 4.5 μm, but the plate-like degree of the tungsten carbide particles is significantly reduced.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing plate-like tungsten carbide powder, characterized in that: The steps include: Step S01: ball-milling tungsten trioxide, an organic carbon source, glucose and sodium chloride, and sieving the mixture and the grinding balls to obtain a mixed powder A; Step S02: putting the mixed powder A into a high-purity graphite crucible, and placing it in a calcining furnace, calcining it at high temperature under an inert gas atmosphere, keeping the temperature, and cooling it to room temperature to obtain a calcined product B; Step S03: washing and filtering the calcined product B to obtain a carbonized material C; Step S04: drying the carbide material C to obtain plate-like tungsten carbide powder; Wherein, in the step S01, the mass ratio of the tungsten trioxide, the organic carbon source, the glucose and the sodium chloride is 1:(1-1.5):(0-0.05):(0.25-1).

2. The method for preparing plate-like tungsten carbide powder according to claim 1, characterized in that: In the step S01, the organic carbon source is at least one of dicyandiamide and melamine.

3. The method for preparing plate-like tungsten carbide powder according to claim 1, characterized in that: In the step S01, the ball-to-material ratio of the ball-milling mixing treatment is (1-3):1, and the ball-milling time is 6-12 hours.

4. The method for preparing plate-like tungsten carbide powder according to claim 1, characterized in that: In the step S02, the high temperature calcination temperature is 1180-1200°C, and the heat preservation time is 2-6 hours.

5. The method for preparing plate-like tungsten carbide powder according to claim 1, characterized in that: The high temperature calcination is divided into two stages. In the first stage, the temperature is raised to 700° C. at 2° C. / min and kept at this temperature for 0.5 h. In the second stage, the temperature is raised to 1180-1200° C. at 2° C. / min and kept at this temperature for 2-6 h.

6. The method for preparing plate-like tungsten carbide powder according to claim 1, characterized in that: In the step S03, the calcined product B is filtered 3 to 5 times with deionized water.

7. The method for preparing plate-like tungsten carbide powder according to claim 1, characterized in that: In the step S04, the drying temperature is 60-100° C., and the drying time is 2-6 hours.

8. The method for preparing plate-like tungsten carbide powder according to claim 1, characterized in that: In the step S02, the inert gas is argon, and the flow rate of the argon introduced into the calcining furnace is controlled to be 100-300 ml / min.

9. The method for preparing plate-like tungsten carbide powder according to claim 1, characterized in that: In the step S01, a 40-80 mesh screen is used to screen the ball-milled mixture.

10. A plate-like tungsten carbide powder, characterized in that: The plate-like tungsten carbide powder is prepared by the method for preparing the plate-like tungsten carbide powder according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Method for preparing hard alloy containing slab-shaped tungsten carbide crystal grain

    CN101117673A

  • Preparation method of nanometer WC whisker

    CN103922341A

  • (W,Mo2)C-Al2O3 composite powder and preparing method thereof

    CN108103344A

  • Preparation method and application of N, S-double-hetero-carbon supported tungsten-based catalyst

    CN114130413A

  • Method for electrocatalytic oxidation of sulfur dioxide by tungsten carbide nano array electrode and application

    CN115233251A

Cited By

  • Two-dimensional tungsten carbide nanosheet loaded non-noble metal catalyst as well as preparation and application thereof

    CN119736662A

  • Plate-shaped ultra-coarse tungsten carbide and preparation method thereof

    CN120172410A