Sunscreen silicon dioxide core-shell particle, preparation method and application thereof

Through the preparation method of silica core-shell particles without surfactant, the problems of poor mechanical strength and environmental impact of sunscreen packaging materials are solved, and efficient and lasting sun protection effect and environmentally friendly preparation process are achieved.

CN118723997APending Publication Date: 2024-10-01NINGBO DILATO MATERIALS CO LTD

Patent Information

Application Number
CN202410719207.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The mechanical strength of existing sunscreen packaging materials is poor, and a large number of small molecule surfactants are required during the preparation process, which affects the environment, and the direct contact between sunscreen and skin may lead to damage.

Method used

The preparation method of silica core-shell particles without surfactant is adopted. The polyalkoxysiloxane precursor is formed by mixing silane, solvent and water and catalyst heating reaction, and the polyalkoxysiloxane precursor is mixed, sunscreen is emulsified, and the pH is adjusted. Wash and dry to obtain silica microcapsules with core-shell structure.

Benefits of technology

It achieves environmentally friendly and efficient preparation, improves the covering properties and sun protection effect of sunscreen, avoids direct contact between sunscreen and skin, extends the sun protection time, and improves the mechanical strength and high temperature resistance of microcapsules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723997A_ABST
    Figure CN118723997A_ABST
Patent Text Reader

Abstract

The invention relates to a sunscreen silicon dioxide core-shell particle and a preparation method and application thereof. The sunscreen silica core-shell particle has a core-shell structure, the shell is formed by silica, the core is a sunscreen agent, and the sunscreen silica core-shell particle does not contain a surfactant. The silicon dioxide microcapsule is wide in size controllable range, the shell material is high in mechanical strength, high in pressure bearing capacity, resistant to high temperature, resistant to flame and resistant to solvent corrosion, the sun-screening agent can be effectively protected, and the sun-screening agent is prevented from being leaked and directly making contact with the skin of the human body. The preparation method of the sunscreen silicon dioxide core-shell particle is simple and efficient, does not need a surfactant, can stabilize emulsification of oily sunscreen molecules in water by using a polyalkoxy siloxane precursor, and is environment-friendly and lower in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to silicon dioxide core-shell particles for sunscreen and a preparation method thereof, in particular to silicon dioxide core-shell particles for sunscreen without surfactant and a preparation method thereof. Background Art

[0002] When people are exposed to the outdoors for a long time, when the skin is overexposed to ultraviolet rays, it will damage epidermal cells, activate tyrosinase, accelerate the synthesis of pigments, cause skin melanization, and destroy the skin's moisturizing function, making the skin dry, damaging the elastic fibers in the dermis, causing fine lines, and causing skin inflammation and burns. Ultraviolet radiation also produces active oxygen and nitrogen, which may cause changes in proteins and DNA in the human body, leading to premature aging of the skin and excessive wrinkles on the skin, and even induce skin cancer. Therefore, sun protection is of great significance to people's appearance and health. Although many physical sun protection methods, such as wearing sun protection clothing, sun hats, and holding parasols, can block ultraviolet rays well, they are limited by the scene and sometimes affect people's activities. Therefore, using sunscreen in skin care products and making them into sunscreen and other products can be more convenient for people to use, and the market recognition is very high.

[0003] Existing sunscreens can be divided into two categories: inorganic sunscreens and organic sunscreens. Inorganic sunscreens protect against the sun by absorbing, reflecting, and scattering ultraviolet rays; organic sunscreens consume energy by destroying hydrogen bonds, opening chelate rings, or tautomerism of molecules under ultraviolet rays, and convert ultraviolet light into harmless heat energy. However, many experiments have shown that direct contact between sunscreen and skin may penetrate the skin and cause new damage to the skin. Therefore, it is necessary to avoid direct contact between sunscreen and human skin.

[0004] The technology of encapsulating sunscreen can effectively block the direct contact between sunscreen and human skin, and improve the safety of use. In addition, by encapsulating sunscreen, the loss of sunscreen can be reduced, the sunscreen effect can be improved, and the sunscreen time can be extended. At present, organic polymers or natural polymers are generally used as encapsulation materials in the industry. For example, patent publication CN114931515 discloses the technology of encapsulating sunscreen with animal wax or plant wax, and patent publication CN115025004 discloses the method of preparing polymer microspheres encapsulating sunscreen by suspension polymerization with ethylene glycol dimethacrylate and surfactant; patent publication CN103169625 uses surfactant to encapsulate sunscreen with substances such as agar, cellulose, and chitosan. However, the mechanical strength of these organic encapsulation materials is usually poor, and a large amount of small molecule surfactants are usually required in the preparation process, which has a certain impact on the environment.

[0005] Silica has excellent mechanical properties, thermal stability and solvent corrosion resistance, as well as good biosafety, making it very suitable as an encapsulation material for sunscreens. The current mainstream silica microcapsules are usually prepared by the emulsion template method, which requires the use of a large amount of surfactants and has certain toxicity. There are certain risks in using them directly in skin care products and other fields.

[0006] Therefore, there is an urgent need for a silicon dioxide product encapsulating a sunscreen agent, and it is hoped that the preparation method thereof is simple and efficient, the synthesis process and the preparation process are environmentally friendly, and the sunscreen agent has good coating properties and a long-lasting sunscreen effect. Summary of the invention

[0007] After in-depth research on the above-mentioned technical problems, the inventors found that by adopting the preparation method of the sunscreen silica core-shell particles of the present invention, the sunscreen silica core-shell particles without surfactant of the present invention can be prepared, the preparation method is simple and efficient, the synthesis process and the preparation process are environmentally friendly, and the sunscreen agent has good coating properties and the sunscreen effect is durable.

[0008] One object of the present invention is to provide a silicon dioxide core-shell particle for sunscreen, which does not contain a surfactant so that the synthesis process and the preparation process are environmentally friendly, and the sunscreen agent has good coating and long-lasting sunscreen effect.

[0009] Another object of the present invention is to provide a method for preparing sunscreen silica core-shell particles, which does not use surfactants, has an environmentally friendly synthesis process and preparation process, and can simply and efficiently prepare sunscreen silica core-shell particles.

[0010] Another object of the present invention is to provide the use of sunscreen silica core-shell particles for preparing cosmetics and skin care products.

[0011] In order to achieve the above object, the present invention provides the following technical solutions:

[0012] [1] A silica core-shell particle for sunscreen, which has a core-shell structure, wherein the shell is formed of silica, the core contains a sunscreen agent, and the silica core-shell particle for sunscreen does not contain a surfactant.

[0013] [2] The sunscreen silica core-shell particles according to [1], wherein the size of the core-shell particles is 100 nm to 10 μm; the shell is dense silica with a thickness of 10 to 500 nm, and the hydroxyl density on the surface of the shell is 1 to 4 / nm 2 .

[0014] [3] The sunscreen silica core-shell particles according to [1] or [2], wherein the sunscreen agent occupies 10 to 95% of the volume of the microcapsule formed by the shell.

[0015] [4] A method for preparing silicon dioxide core-shell particles for sunscreen, comprising the following steps:

[0016] Step 1: Silane, solvent and water are fully mixed, a catalyst is added, and after the heating reaction is complete, by-products and solvent are removed by distillation to obtain a polyalkoxysiloxane precursor;

[0017] Step 2: mixing the polyalkoxysiloxane precursor obtained in step 1 and the sunscreen agent to form a mixed liquid;

[0018] Step 3: emulsifying the mixed solution obtained in step 2, adding alkali solution to adjust the emulsion to a pH of 8 to 12 for reaction, and then washing and separating to remove impurities and by-products to obtain an aqueous dispersion of silicon dioxide core-shell particles for sunscreen;

[0019] Step 4: Drying the aqueous dispersion to obtain sunscreen silica core-shell particle powder.

[0020] [5] The preparation method according to [4], wherein the silane used in step 1 is a monomer having the following chemical formula, or a polysiloxane precursor having a silicon dioxide content of less than 60%;

[0021] R 1 n -Si-(OR 2 ) (4-n)

[0022] Among them, R 1 is at least one non-hydrolyzable group selected from unsubstituted alkyl, vinyl alkyl, epoxy alkyl, styryl alkyl, (meth)acryloxy alkyl, amino alkyl, urea alkyl, chloropropyl alkyl, haloalkyl, isocyanate alkyl or hydroxyalkyl, R 2 is an alkyl group having 1 to 6 carbon atoms; n is 0, 1 or 2; each R 2 are the same or different from each other; when n is 2, each R 1 The same as or different from each other.

[0023] [6] The preparation method according to [4], wherein the solvent in step 1 is at least one selected from methanol, ethanol, isopropanol, butanol, ethylene glycol, ethylene glycol butyl ether, propylene glycol, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, acetone, and butanone, and the weight ratio of the solvent to the silane is (0.1-10):1;

[0024] The molar concentration of the catalyst in the step 1 is 0.01-10 mol / L, and the weight ratio of the catalyst to the silane is (0.001-0.2):1;

[0025] The catalyst in step 1 is at least one selected from hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, acidic cation exchange resin, aluminum trichloride, boron trifluoride, and alkoxytitanium.

[0026] [7] The preparation method according to [4], wherein the temperature of the heating reaction in step 1 is 30 to 100°C, the reaction time is 1 to 24 hours, and the distillation is selected from one or a combination of atmospheric distillation, reduced pressure distillation, thin film evaporation or rotary evaporation.

[0027] [8] The preparation method according to [4], wherein the sunscreen in step 2 is at least one selected from p-methoxycinnamate, camphor derivatives, benzotriazoles and octocrylene.

[0028] [9] The preparation method according to [4], wherein the separation in step three is centrifugation, filtration, ultrafiltration or dialysis.

[0029]

[10] Use of the sunscreen silica core-shell particles according to any one of [1] to [3] for preparing cosmetics and skin care products.

[0030] Effects of the Invention

[0031] The method for preparing the sunscreen silicon dioxide core-shell particles of the present invention is simple and efficient, does not require a surfactant, and can stabilize the emulsification of oily sunscreen molecules in water by using a polyalkoxysiloxane precursor, is environmentally friendly, and has lower costs.

[0032] The silica microcapsules of the present invention have a wide controllable size range, a high mechanical strength of the shell material, a strong pressure bearing capacity, and are resistant to high temperatures, flame retardant, and solvent corrosion, and can effectively protect the sunscreen and prevent it from leaking and directly contacting human skin.

[0033] The silicon dioxide microcapsules of the present invention can be applied to the coating of most organic sunscreens and have a high coating efficiency, and can be widely used in various daily chemical products to effectively protect the skin from suntan and sunburn. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is the particle size distribution diagram of the silicon dioxide core-shell particles for sunscreen prepared in Example 1.

[0035] Figure 2 This is the particle size distribution diagram of the silicon dioxide core-shell particles for sunscreen prepared in Example 2.

[0036] Figure 3 This is the particle size distribution diagram of the silicon dioxide core-shell particles for sunscreen prepared in Example 3.

[0037] Figure 4The release curves of the sunscreen agent in the sunscreen silica core-shell particles prepared in Examples 1 to 3.

[0038] Figure 5 The figure is a relationship diagram between the SPF value and the sunscreen content of the sunscreen prepared in Application Example 1 and Comparative Example 1.

[0039] Figure 6 The SPF value variation curve of the sunscreen (sunscreen content is 10 wt %) prepared in Application Example 1 and Comparative Example 1 within 12 hours. DETAILED DESCRIPTION

[0040] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the scope of the present invention is not limited in any way. Unless otherwise stated, the reagents used in the specific examples can be obtained through commercial means or conventional experimental means.

[0041] [Silica core-shell particles for sunscreen]

[0042] The sunscreen silica core-shell particles of the present invention have a core-shell structure, wherein the shell is formed by silica, the core is a sunscreen agent, and the sunscreen silica core-shell particles do not contain a surfactant. Since they do not contain a surfactant, they are environmentally friendly.

[0043] The size of the silica core-shell particles for sunscreen of the present invention may be, for example, 100 nm to 10 μm. In some embodiments of the silica core-shell particles for sunscreen, the shell is, for example, a dense silica with a thickness of 10 to 500 nm, and the surface of the shell has 1 to 4 nanoparticles / nm. 2 The hydroxyl density.

[0044] In some embodiments of the sunscreen silica core-shell particles, the volume of the sunscreen agent in the microcapsule formed by the shell is, for example, in the range of 10% to 95%. By setting the volume of the sunscreen agent in the microcapsule formed by the shell to be 10% or more, the sunscreen silica core-shell particles can have sufficient sunscreen agent to achieve a sufficient sunscreen effect.

[0045] The silicon dioxide core-shell particles for sunscreen can be prepared by the following method for preparing silicon dioxide core-shell particles for sunscreen.

[0046] [Preparation method of silicon dioxide core-shell particles for sunscreen]

[0047] The preparation method of the sunscreen silicon dioxide core-shell particles of the present invention comprises the following steps:

[0048] Step 1: Silane, solvent and water are fully mixed, a catalyst is added, and after the heating reaction is complete, by-products and solvent are removed by distillation to obtain a polyalkoxysiloxane precursor;

[0049] Step 2: mixing the polyalkoxysiloxane precursor obtained in step 1 and the sunscreen agent to form a mixed liquid;

[0050] Step 3: emulsifying the mixed solution obtained in step 2, adding alkali solution to adjust the emulsion to a pH of 8 to 12 for reaction, and then washing and separating to remove impurities and by-products to obtain an aqueous dispersion of silicon dioxide core-shell particles for sunscreen;

[0051] Step 4: Drying the aqueous dispersion to obtain sunscreen silica core-shell particle powder.

[0052] In the method for preparing the silica core-shell particles for sunscreen according to some embodiments, the silane used in the aforementioned step 1 is, for example, a monomer having the following chemical formula, or a polysiloxane precursor having a silica content of 60% or less;

[0053] R 1 n -Si-(OR 2 ) (4-n)

[0054] Among them, R 1 is at least one non-hydrolyzable group selected from unsubstituted alkyl, vinyl alkyl, epoxy alkyl, styryl alkyl, (meth)acryloxy alkyl, amino alkyl, urea alkyl, chloropropyl alkyl, haloalkyl, isocyanate alkyl or hydroxyalkyl, R 2 is an alkyl group having 1 to 6 carbon atoms; n is 0, 1 or 2; each R 2 are the same or different from each other; when n is 2, each R 1 The same as or different from each other.

[0055] In some embodiments of the method for preparing the sunscreen silica core-shell particles, the solvent used in the aforementioned step 1 may be, for example, at least one selected from methanol, ethanol, isopropanol, butanol, ethylene glycol, ethylene glycol butyl ether, propylene glycol, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, acetone, and butanone. Regarding the amount of the solvent, it is preferred that the weight ratio of the solvent to the silane is in the range of (0.1 to 10):1.

[0056] In the above step 1, the molar concentration of the catalyst can be, for example, 0.01 to 10 mol / L. Regarding the amount of the catalyst, the weight ratio of the catalyst to the silane can be, for example, (0.001 to 0.2):1.

[0057] Examples of the catalyst used in the step 1 include at least one selected from hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, an acidic cation exchange resin, aluminum trichloride, boron trifluoride, and titanium alkoxide.

[0058] In some embodiments of the method for preparing sunscreen silica core-shell particles, the temperature of the heating reaction in the aforementioned step 1 can be, for example, 30 to 100° C., and the reaction time can be, for example, 1 to 24 hours. The distillation in the aforementioned step 1 can be, for example, one selected from atmospheric distillation, reduced pressure distillation, thin film evaporation, or rotary evaporation, or a combination thereof.

[0059] In some embodiments of the method for preparing sunscreen silica core-shell particles, the sunscreen used in step 2 may include at least one selected from the group consisting of p-methoxycinnamate, camphor derivatives, benzotriazoles, and octocrylene.

[0060] In some embodiments of the method for preparing the sunscreen silica core-shell particles, the separation in the aforementioned step three may include, for example, centrifugal separation, filtration, ultrafiltration or dialysis.

[0061] In some embodiments of the method for preparing sunscreen silica core-shell particles, the drying in the aforementioned step 4 includes but is not limited to oven drying, freeze drying, spray drying, etc.

[0062] [Use of silicon dioxide core-shell particles for sunscreen in the preparation of cosmetics and skin care products]

[0063] The sunscreen silica core-shell particles of the present invention can be used for preparing cosmetics, skin care products and the like.

[0064] Example

[0065] Example 1

[0066] 160g of tetraethyl orthosilicate condensate (T40) and 48g of anhydrous ethanol are mixed evenly, and then 14g of hydrochloric acid with a mass fraction of 37% and 12g of deionized water are added respectively and mixed evenly, the temperature is raised to 80°C and the reaction is continued for 2 hours, and the solvent and low molecular weight compounds in the system are distilled off by rapid rotation under reduced pressure to obtain a transparent polyalkoxysiloxane precursor with a certain viscosity and flowability; 12g of the polyalkoxysiloxane precursor, 9g of octyl methoxycinnamate and 3g of avobenzone are added to 300g of deionized water; emulsification is performed by a homogenizer at 12000rpm for 5 minutes to obtain a white emulsion; 10g of ammonia water (concentration 25%) is added, and the emulsion is continuously magnetically stirred for 12 hours to obtain a milky white sunscreen silica core-shell particle dispersion slurry; most of the water is removed by centrifugation, and further dried by freeze drying to obtain a white sunscreen silica core-shell particle powder. Thermogravimetric analysis showed that the thermal weight loss of the microcapsules at 800°C was 67%. According to the calculation based on the feed, the encapsulation rate was close to 100%. The particle size distribution of the sunscreen silica core-shell particles prepared in Example 1 was measured by dynamic light scattering. The results are shown in Figure 1 .from Figure 1It can be seen that the average particle size of the sunscreen silica core-shell particles prepared in Example 1 is 667 nm, and the particle size distribution index is 0.256.

[0067] Furthermore, the sunscreen silica core-shell particle powder synthesized in Example 1 (the mass percentage of sunscreen in the sunscreen silica core-shell particle powder is 45%) was mixed with a commercially available moisturizing cream so that the mass percentage of the sunscreen after mixing was 3wt%, 5wt%, 7wt% and 10wt%, respectively. After stirring evenly, a series of sunscreens were obtained.

[0068] Example 2

[0069] 160g of ethyl orthosilicate condensate (T40) in step 1 of Example 1 was replaced with 150g of tetraethyl orthosilicate and 38g of methyltriethoxysilane, and the rest was prepared in the same manner as in Example 1. Thermogravimetric analysis of the sunscreen silica core-shell particles prepared in Example 2 showed a thermal weight loss of 62% at 800°C. Based on the feed calculation, the encapsulation rate was 92%. In addition, the particle size distribution of the sunscreen silica core-shell particles prepared in Example 2 was measured by a dynamic light scattering instrument, and the results are shown in Figure 2 .from Figure 2 It can be seen that the average particle size is 3455 nm and the particle size distribution index is 0.375.

[0070] Example 3

[0071] 160g of tetraethyl orthosilicate condensate (T40) in step 1 of Example 1 was replaced by 150g of tetraethyl orthosilicate and 38g of methyltriethoxysilane, and 12g of polyalkoxysiloxane precursor in step 2 was replaced by 9g of polyalkoxysiloxane precursor. The rest was prepared in the same manner as in Example 1. Thermogravimetric analysis of the sunscreen silica core-shell particles prepared in Example 3 showed that the thermal weight loss at 800°C was 86%, and the encapsulation rate was 96% based on the feed.

[0072] In addition, the particle size distribution of the sunscreen silica core-shell particles prepared in Example 3 was measured by dynamic light scattering. The results are shown in Figure 3 .from Figure 3 It can be seen that the average particle size is 1233 nm and the particle size distribution index is 0.276.

[0073] Sunscreen release curve determination:

[0074] The release behavior of the sunscreen silicon dioxide core-shell particles prepared in Examples 1 to 3 within 24 hours was tested by dialysis method. The results are as follows: Figure 4 As shown. Figure 4It can be seen that the release rate of the sunscreen silica core-shell particles prepared in Examples 1 to 3 is slow, and within 24 hours, the relative release rate of the sunscreen agent decreases from 75% to 21.7%, 18.2% and 27.6%, respectively, indicating that the sunscreen silica core-shell particles prepared in Examples 1 to 3 effectively maintain a sunscreen effect for more than 24 hours.

[0075] Comparative Example 1

[0076] The sunscreen (octyl methoxycinnamate and avobenzone mixed in a ratio of 3:1) was mixed with a commercially available moisturizing cream according to the mass percentage of the mixed sunscreen after 0, 3wt%, 5wt%, 7wt% and 10wt% respectively, and after stirring evenly, a series of sunscreens were obtained.

[0077] Sunscreen performance test

[0078] The SPF values ​​of the sunscreens prepared in Example 1 and Comparative Example 1 were tested. The results are as follows: Figure 5 shown.

[0079] Time-dependent SPF test

[0080] The change in SPF value of the sunscreen with a mass percentage of 10 wt% of the sunscreen prepared in Application Example 1 within 12 hours was measured. The results are as follows: Figure 6 shown.

[0081] from Figure 5 , Figure 6 It can be seen that compared with the sunscreen obtained by directly adding the sunscreen agent, the sunscreen effect and sunscreen duration of the sunscreen prepared by using the sunscreen silica core-shell particles prepared in Example 1 are significantly improved.

[0082] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the invention disclosed herein. The present invention is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary technical means in the art that are not disclosed by the present invention.

Claims

1. A silicon dioxide core-shell particle for sunscreen, It is characterized in that The sunscreen silica core-shell particles have a core-shell structure, the shell is formed of silicon dioxide, the core contains a sunscreen agent, and the sunscreen silicon dioxide core-shell particles do not contain a surfactant.

2. The sunscreen silica core-shell particles according to claim 1, in, The size of the core-shell particles is 100nm to 10μm; the shell is dense silica with a thickness of 10 to 500nm, and the hydroxyl density on the surface of the shell is 1 to 4 / nm 2 .

3. The sunscreen silica core-shell particles according to claim 1 or 2, in, The sunscreen agent occupies 10 to 95% of the volume of the microcapsule formed by the shell.

4. A method for preparing the sunscreen silica core-shell particles according to any one of claims 1 to 3, It is characterized in that Including the following processes: Step 1: Silane, solvent and water are fully mixed, a catalyst is added, and after the heating reaction is complete, by-products and solvent are removed by distillation to obtain a polyalkoxysiloxane precursor; Step 2: mixing the polyalkoxysiloxane precursor obtained in step 1 and the sunscreen agent to form a mixed liquid; Step 3: emulsifying the mixed solution obtained in step 2, adding alkali solution to adjust the emulsion to a pH of 8 to 12 for reaction, and then washing and separating to remove impurities and by-products to obtain an aqueous dispersion of silicon dioxide core-shell particles for sunscreen; Step 4: Drying the aqueous dispersion to obtain sunscreen silica core-shell particle powder.

5. The preparation method according to claim 4, in, The silane used in the step 1 is a monomer having the following chemical formula, or a polysiloxane precursor having a silicon dioxide content of less than 60%; R 1 n -Si-(OR 2 ) (4-n) Among them, R 1 is at least one non-hydrolyzable group selected from unsubstituted alkyl, vinyl alkyl, epoxy alkyl, styryl alkyl, (meth)acryloxy alkyl, amino alkyl, urea alkyl, chloropropyl alkyl, haloalkyl, isocyanate alkyl or hydroxyalkyl, R 2 is an alkyl group having 1 to 6 carbon atoms; n is 0, 1 or 2; each R 2 are the same or different from each other; when n is 2, each R 1 The same as or different from each other.

6. The preparation method according to claim 4, in, The solvent in the step 1 is at least one selected from methanol, ethanol, isopropanol, butanol, ethylene glycol, ethylene glycol butyl ether, propylene glycol, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, acetone, and butanone, and the weight ratio of the solvent to the silane is (0.1-10):1; The molar concentration of the catalyst in the step 1 is 0.01-10 mol / L, and the weight ratio of the catalyst to the silane is (0.001-0.2):1; The catalyst in step 1 is at least one selected from hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, acidic cation exchange resin, aluminum trichloride, boron trifluoride, and alkoxytitanium.

7. The preparation method according to claim 4, in, The temperature of the heating reaction in the step 1 is 30-100° C., the reaction time is 1-24 hours, and the distillation is selected from one of atmospheric distillation, reduced pressure distillation, thin film evaporation or rotary evaporation or a combination thereof.

8. The preparation method according to claim 4, in, The sunscreen in step 2 is at least one selected from p-methoxycinnamate, camphor derivatives, benzotriazoles and octocrylene.

9. The preparation method according to claim 4, in, The separation in step three is centrifugal separation, filtration, ultrafiltration or dialysis.

10. Use of the sunscreen silica core-shell particles according to any one of claims 1 to 3 for preparing cosmetics and skin care products.

Citation Information

Patent Citations

  • Methods for preparing microencapsulated sunscreens, microencapsulated sunscreens, and sunscreen products containing the same.

    CN114931515A

  • Sunscreen microcapsule as well as preparation method and application thereof

    CN115025004A

Cited By

  • Supramolecular double-gating photoresponse mesoporous silicon sunscreen composite material as well as preparation method and application thereof

    CN122849068A