Method for removing carbonate in lithium hydroxide production process
By detecting and controlling the carbonate content, using the reaction of acid and alkali and the design of the buffer tank, the problem of carbonate scaling in the production of lithium hydroxide is solved, the stability and energy consumption efficiency of the evaporator are improved, and efficient carbonation is achieved. Root removal.
Patent Information
- Application Number
- CN202410638835.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing lithium hydroxide production process, carbonate scaling occurs during the evaporation process after calcium removal, causing the evaporator pipeline to be blocked, affecting evaporation efficiency and production stability.
By detecting the carbonate content of the decalcified liquid and calculating the acid flow and molecular weight according to a specific formula, acid is added to the decalcified liquid for reaction, the pH value is controlled to about 4, and alkali is added to operate until it is above neutral. , combined with the insulation of the buffer tank and the design of the evaporator, to ensure the removal of carbonate and product stability.
It effectively reduces the fouling of the evaporator, improves production stability and energy consumption efficiency, ensures that the carbonate removal rate is above 80%, reduces energy consumption, and enhances market competitiveness.
Smart Images

Figure CN118724022A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium hydroxide production, and in particular to a method for removing carbonate in a lithium hydroxide production process. Background Art
[0002] In the process of extracting lithium salts by the prior art, since spodumene, lepidolite and other minerals are basically used as raw materials for production, the content of impurity metals in the production materials is relatively high (such as iron, magnesium, aluminum, calcium, etc.). In order to ensure the excellence of the final product indicators, it is inevitable to use other chemical auxiliary materials for impurity removal. Among them, in order to remove metallic calcium, the auxiliary material mainly used is sodium carbonate, which is generated by reaction and filtered out. However, in order to ensure the removal efficiency of metallic calcium, the addition of sodium carbonate will be excessive, resulting in too high a carbonate ion in the material. In the subsequent production process, especially in the evaporation process after decalcification, lithium carbonate with low solubility will be generated, and crystallization will cause scaling and clogging of the pipeline, affecting the stable operation and evaporation efficiency of the evaporator, and having a great impact on the product output, product indicator stability, and energy consumption control of the entire production process.
[0003] However, there is no method for removing carbonate in the current lithium salt extraction technology. Therefore, scaling occurs during the evaporation process after decalcification, causing blockage of the evaporator pipeline, affecting the evaporation efficiency and production stability. Summary of the invention
[0004] The object of the present invention is to provide a method for removing carbonate in a lithium hydroxide production process, so as to solve the technical problem that scaling occurs in the evaporation process after decalcification in the prior art, resulting in blockage of the evaporator pipeline and affecting the evaporation efficiency and production stability.
[0005] The present invention discloses a method for removing carbonate in a lithium hydroxide production process, comprising the following steps:
[0006] S1. Detecting the carbonate content of the decalcified liquid;
[0007] S2. Add acid to the decalcified liquid according to the formula:
[0008]
[0009] In the formula, F is the hourly flow rate of the acid used, x is the carbonate content of the decalcified liquid, y is the designed hourly processing volume of the decalcified liquid, a is the molecular weight of the acid used, b is the density of the acid used, c is the hydroxide concentration of the decalcified liquid, d is the number of hydrogen ions contained in the acid used, and z is the removal coefficient, which ranges from 2 to 2.2.
[0010] Furthermore, the decalcified liquid first enters the decarbonated liquid buffer tank, and then enters the decarbonated liquid reaction tank to add acid for reaction. The decarbonated liquid buffer tank here plays a role of buffering and heat preservation, preventing the decalcification process from shutting down and the output flow rate from being too low, which affects the subsequent production.
[0011] Furthermore, the temperature in the pre-liquid buffer tank for removing carbonate is maintained at 40-50°C. Insulating the pre-liquid buffer tank for removing carbonate can prevent the material from cooling too quickly, causing carbon dioxide in the air to be adsorbed into the material, thereby causing an increase in carbonate. The solubility of lithium carbonate decreases with increasing temperature. Although the carbonate content in the material is low at too high a temperature, there is a risk of crystallization blocking the pipeline due to the decrease in the solubility of lithium carbonate.
[0012] Furthermore, when the level of the decalcified liquid in the reaction tank is 70% of the volume of the reaction tank, acid is added. After the acid is added, a violent double decomposition reaction will occur to produce a large amount of gas (CO3 2- +2H + =H2O+CO2↑). If the material level is high, there will be a risk of the reaction tank bubbling.
[0013] Furthermore, the acid is reacted for 5-10 minutes after being added. If it is less than 5 minutes, the removal efficiency cannot be achieved, and if it is more than 10 minutes, the reaction efficiency decreases. Although the removal efficiency is increased, the production efficiency is also reduced.
[0014] Furthermore, after the acid addition reaction is completed, the pH is monitored. If the pH is not greater than 4, the next step is performed. If the pH is greater than 4, acid is added again according to the formula until the pH is no greater than 4 and the reaction is stopped.
[0015] Furthermore, the alkali addition operation is performed after the pH is no greater than 4.
[0016] Furthermore, the alkali addition operation adjusts the pH to above neutral. Because dilute acid is particularly corrosive to equipment and pipelines, the pH needs to be adjusted to above neutral to avoid safety accidents.
[0017] Furthermore, the alkali addition operation adjusts the pH to 8.
[0018] Furthermore, after the alkali addition operation is completed, the material is sent to a post-carbonation removal liquid buffer tank, and the post-carbonation removal liquid buffer tank is insulated and protected. By insulating the post-carbonation removal liquid buffer tank, the heat exchange of the material is reduced, and the carbon dioxide in the air is prevented from being adsorbed into the material due to the low temperature of the material, so that the carbonate of the material increases. At the same time, the insulation here can increase the temperature of the material when it enters the evaporator, reduce the heat exchange temperature difference of the evaporator, and thus achieve energy saving effect.
[0019] Furthermore, the material in the liquid buffer tank after the removal of carbonate is sent to an evaporator.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The present invention aims at the problems of unstable production operation, high evaporator energy consumption, unstable product indicators, etc. caused by evaporator scaling in the production process of lithium hydroxide. After debugging, the evaporator scaling is effectively reduced while ensuring the production output, and at the same time, the stability of product indicators is played a good role;
[0022] 2. The present invention calculates and verifies parameter settings, adopts DCS automatic control, and interlocks the pH meter of the carbonate removal reaction tank with the acid addition flow rate. While ensuring low auxiliary material consumption, the carbonate removal rate can reach more than 80%, while effectively ensuring the stability of the product carbonate index, reducing energy consumption, and significantly improving market competitiveness. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only represent some embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0024] Figure 1 This is a schematic diagram of the carbonate index trend in Example 1 of the present invention.
[0025] Figure 2 This is a schematic diagram of the carbonate index trend in Example 2 of the present invention.
[0026] Figure 3 This is a schematic diagram of the carbonate index trend in Example 3 of the present invention. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0028] Example 1
[0029] The method for removing carbonate in a lithium hydroxide production process of the above-mentioned device used in this embodiment comprises the following steps:
[0030] S1. The decalcified liquid first enters the pre-carbonate liquid buffer tank, the pre-carbonate liquid buffer tank temperature is maintained at 40-50 ° C, and then enters the carbonate removal reaction tank to detect the carbonate content of the decalcified liquid;
[0031] S2. Add acid to the decalcified liquid according to the formula:
[0032]
[0033] In the formula, F is the hourly flow rate of the acid used, x is the carbonate content of the decalcified liquid, y is the designed hourly processing volume of the decalcified liquid, a is the molecular weight of the acid used, b is the density of the acid used, c is the hydroxide concentration of the decalcified liquid, d is the number of hydrogen ions contained in the acid used, and z is the removal coefficient, which ranges from 2 to 2.2.
[0034] In this embodiment:
[0035]
[0036] but:
[0037] The amount of sulfuric acid consumed by carbonate ion: 2g / l*35000L÷60*98.08÷1.85÷1000=61.85L;
[0038] The amount of sulfuric acid consumed by hydroxide (pH of the solution after decalcification = 12, hydroxide concentration 0.01 mol / L): 0.01 mol / L*35000L÷2*98.08÷1.85÷1000=9.28L;
[0039] Adjust pH to 4 (hydrogen ion concentration 0.0001 mol / L) Sulfuric acid consumption: 0.0001 mol / L*35000L÷2*98.08÷1.85÷1000=0.09L
[0040] Theoretically, the total amount of 98% sulfuric acid required is: (61.85+9.28+0.09) L / h÷98%=72.67 L / h
[0041] Since the expected carbonate removal efficiency cannot be achieved within a short reaction time after adding the theoretical acid addition amount, the actual acid addition amount needs to increase a removal coefficient, which is 2-2.2;
[0042] In this example, the removal coefficient z is 2.1, so the actual amount of sulfuric acid added is:
[0043] 72.67L / h*2.1=152.61L / h.
[0044] S3. When the level of the decalcified liquid in the reaction tank reaches 70% of the volume of the reaction tank, acid addition begins.
[0045] S4. After the acid is added, react for 5 minutes. After the reaction is completed, monitor the pH. If the pH is not greater than 4, proceed to the next step. If the pH is greater than 4, add acid again according to the formula until the pH is no greater than 4 and stop.
[0046] S5. After the pH value is not greater than 4, add alkali to adjust the pH value to 8. After the alkali addition operation is completed, send the material to the post-carbonate removal liquid buffer tank and finally to the evaporator.
[0047] Example 2
[0048] In this embodiment, as a preferred embodiment of the present invention, a method for removing carbonate in a lithium hydroxide production process is provided, which is different from Example 1 except that the carbonate content of the liquid after decalcification is 1.8 g / l.
[0049] Example 3
[0050] In this embodiment, as a preferred embodiment of the present invention, a method for removing carbonate in a lithium hydroxide production process is provided, which is different from Example 1 in that the carbonate content of the liquid after decalcification is 2.2 g / l.
[0051] Comparative Example 1
[0052] In this embodiment, as a comparative example of the present invention, a method for removing carbonate in a lithium hydroxide production process is provided. The only change to Example 1 is that the reaction time after adding acid is 3 minutes.
[0053] After changing the reaction time after acid addition, the carbonate removal efficiency in the material was about (2-1.45) ÷ 2 = 43%, which could not reach the minimum expected removal rate of 60%. At this removal rate, the test showed that the evaporator still had a high frequency of scaling and the evaporator had a high energy consumption, which did not meet the rectification expectations.
[0054] Comparative Example 2
[0055] In this embodiment, as a comparative example of the present invention, a method for removing carbonate ions in a lithium hydroxide production process is used. The only change on the basis of Example 1 is that the amount of acid added is 138.07 L / h (the removal coefficient is 1.9 at this time).
[0056] After reducing the amount of acid added, it can be clearly seen that the efficiency of removing carbonate from the material is reduced in the reaction period of 3-15 minutes, and when the reaction time is 15 minutes, the removal efficiency is only (2-0.66) ÷ 2 = 67%, which is lower than the removal efficiency of (2-0.5) ÷ 2 = 75% when the reaction time is 10 minutes when the removal coefficient is 2.1. At the same time, under this removal coefficient, the scaling frequency of the evaporator is slightly reduced, but the energy consumption of the evaporator has not been greatly improved.
[0057] Table 1 Carbonate content of materials after acid addition
[0058]
[0059] from Figure 1-Figure 3As can be seen from Table 1, too low removal efficiency will lead to lower carbonate removal efficiency and no obvious improvement in evaporator scaling, and no obvious reduction in evaporator energy consumption. Too high removal efficiency will lead to increased acid usage and increased costs. If the reaction time is too short, the carbonate in the material cannot be completely removed and there is no obvious improvement in evaporator scaling, the evaporator energy consumption is high, and too long reaction time will affect the output.
[0060] When the removal coefficient is 2-2.3 and the reaction time is 5-10min, the efficiency of carbonate removal from the material is the highest, the cost is the lowest, and there is no obvious impact on the product. Under this condition, a carbonate removal rate of more than 70% can be achieved, and the scaling and energy consumption of the evaporator can be significantly improved, and it also has a good effect on the stability of the product carbonate index.
[0061] The above are the implementation methods listed in this embodiment, but this embodiment is not limited to the above optional implementation methods. Those skilled in the art can arbitrarily combine the above methods to obtain other various implementation methods. Anyone can derive other various forms of implementation methods under the inspiration of this embodiment. The above specific implementation methods should not be understood as limiting the scope of protection of this embodiment. The scope of protection of this embodiment shall be based on the definition in the claims, and the description can be used to interpret the claims.
Claims
1. A method for removing carbonate in a lithium hydroxide production process, Features: The following steps are involved: S1. Detecting the carbonate content of the decalcified liquid; S2. Add acid to the decalcified liquid according to the formula: In the formula, F is the hourly flow rate of the acid used, x is the carbonate content of the decalcified liquid, y is the designed hourly processing volume of the decalcified liquid, a is the molecular weight of the acid used, b is the density of the acid used, c is the hydroxide concentration of the decalcified liquid, d is the number of hydrogen ions contained in the acid used, and z is the removal coefficient, which ranges from 2 to 2.
2.
2. A method for removing carbonate in a lithium hydroxide production process according to claim 1, Features: The decalcified liquid first enters the pre-carbonate removal liquid buffer tank, and then enters the carbonate removal reaction tank to add acid for reaction.
3. A method for removing carbonate in a lithium hydroxide production process according to claim 2, Features: The temperature in the buffer tank for the pre-carbonate removal solution is maintained at 40-50°C.
4. A method for removing carbonate in a lithium hydroxide production process according to claim 2, Features: When the liquid level of the decalcified liquid in the reaction tank reaches 70% of the volume of the reaction tank, acid addition begins.
5. A method for removing carbonate in a lithium hydroxide production process according to claim 1, Features: The acid is added and reacted for 5-10 minutes.
6. A method for removing carbonate in a lithium hydroxide production process according to claim 5, Features: After the acid addition reaction is completed, the pH is monitored. If the pH is not greater than 4, the next step is performed. If the pH is greater than 4, acid is added again according to the formula until the pH is no greater than 4 and the reaction is stopped.
7. A method for removing carbonate in a lithium hydroxide production process according to claim 6, Features: The alkali addition operation is performed after the pH is no greater than 4.
8. A method for removing carbonate in a lithium hydroxide production process according to claim 7, Features: The alkali addition operation adjusts the pH to above neutral.
9. The method for removing carbonate from a lithium hydroxide production process according to claim 7, Features: After the alkali addition operation is completed, the material is sent to a post-carbonate removal liquid buffer tank, and the post-carbonate removal liquid buffer tank is heat-insulated and protected.