Method for preparing lithium carbonate from carbonate clay type lithium ore
Through multi-step processing of carbonate clay lithium ore, the efficient extraction of lithium element and the separation of various valuable elements are achieved, which solves the problem of low utilization rate of lithium ore resources, reduces energy consumption, and improves lithium resources. The recycling rate and comprehensive utilization rate have filled the technical gap in this field.
Patent Information
- Application Number
- CN202410878908.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-01
AI Technical Summary
Existing technology cannot effectively utilize carbonate clay lithium ore resources, resulting in low lithium ore grade, high energy consumption, and low recovery rate. Domestic lithium resources are heavily dependent on external sources, which affects national energy security.
By crushing, grinding, screening, roasting, acid leaching, impurity removal, enrichment and lithium precipitation of carbonate clay lithium ore, valuable elements are separated step by step to prepare high-purity lithium carbonate.
It achieves efficient and clean utilization of carbonate clay lithium ore resources, reduces production costs, improves the recovery rate and comprehensive utilization rate of lithium resources, fills the technical gap in this field, and reduces dependence on external lithium resources.
Smart Images

Figure CN118724030A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of comprehensive resource utilization, and in particular to a method for preparing lithium carbonate from carbonate clay-type lithium ore. Background Art
[0002] With the development of social economy, the contradiction between supply and demand of global oil resources has become increasingly prominent, and major economies have been promoting and popularizing electric vehicles. Driven by the hybrid and electric vehicle lithium battery market, the global demand for lithium carbonate has increased significantly, and lithium-ion new energy has become one of the energy industries that the country focuses on supporting and developing.
[0003] China has rich resource reserves, but the domestic dependence on foreign raw materials for lithium product processing is as high as 80%, of which imported spodumene accounts for 66% and imported high-concentration brine accounts for 18%. The main reasons for my country's lithium resource imports are: first, the production cost of lithium mica resources in ore extraction of lithium remains high, and spodumene ore resources are difficult to mine geographically, or have poor quality and scattered distribution, which basically cannot meet the long-term needs of lithium carbonate production companies. Therefore, it is necessary to import high-quality lithium concentrate resources from abroad; second, the magnesium-lithium ratio of my country's salt lake brine is high, and the lithium extraction technology is difficult. The technical barriers force domestic companies to import high-concentration brine with a low magnesium-lithium ratio from abroad. Therefore, finding and developing new lithium resources has become a top priority for my country.
[0004] In recent years, carbonate clay-type lithium ore is a new type of lithium ore discovered in the central Yunnan region, with huge resources. However, the work on the efficient, clean and comprehensive utilization of lithium resources in "carbonate clay-type lithium deposits" is still a research and technical gap, with no precedents and research materials for reference.
[0005] At the same time, the existing technology is relatively mature for the extraction of lithium from traditional lithium resources, but it is not yet applicable to the development and utilization of carbonate clay-type lithium ore resources. With the increasing pressure on environmental protection, there is an urgent need for the clean and comprehensive utilization of its resources. If a clean and efficient lithium extraction process from carbonate clay-type lithium ore can be developed, it can fundamentally solve my country's dependence on external lithium resources and ensure national energy security. Summary of the invention
[0006] In view of the above problems existing in the prior art, the present invention provides a method for preparing lithium carbonate from carbonate clay-type lithium ore, which fills the gap in the comprehensive utilization of carbonate clay-type lithium ore, effectively solves the problems of low grade of lithium ore, high energy consumption and low recovery rate, and provides a technical basis for the development and utilization of lithium resources.
[0007] The present invention discloses a method for preparing lithium carbonate from carbonate clay-type lithium ore, comprising:
[0008] The carbonate clay type lithium ore is crushed, ground, screened and roasted in sequence to obtain roasted clinker;
[0009] The roasted clinker is subjected to acid leaching treatment, and then filtered to obtain a leaching solution;
[0010] Adding a neutralizing precipitant to the leaching solution for a first impurity removal treatment, and then filtering to obtain a neutralized filtrate;
[0011] Adding a purification precipitant to the neutralized filtrate to perform a second impurity removal treatment, and then filtering to obtain a purified filtrate;
[0012] Carrying out enrichment treatment on the purified filtrate to obtain an enriched liquid;
[0013] A lithium precipitating agent is added to the enriched solution to obtain lithium carbonate.
[0014] As a further improvement of the present invention, the carbonate clay type lithium ore is crushed, ground, screened and roasted in sequence to obtain roasted clinker; comprising:
[0015] Crushing the carbonate clay type lithium ore to obtain ore material; wherein the particle size of the ore material is 2 mm to 30 mm;
[0016] Grinding the ore to obtain a coarse powder; wherein the grinding time is 10 minutes to 60 minutes;
[0017] The coarse powder is screened to obtain the undersize product; wherein the particle size of the undersize product is less than 0.850 mm, and the oversize product is returned to the grinding section for further grinding, and the mass of the undersize product accounts for 60% to 90%;
[0018] The product under the sieve is roasted to obtain roasted clinker; wherein the roasting temperature is 300°C to 1500°C.
[0019] As a further improvement of the present invention, in the acid leaching process,
[0020] The acid used includes, but is not limited to, one or more of the following: sulfuric acid, hydrochloric acid, nitric acid, acetic acid, citric acid, tartaric acid, oxalic acid;
[0021] The mass fraction of the acid solution is 10% to 30%, and the solid-liquid ratio of the roasted clinker to the acid solution is 1:1 to 1:5;
[0022] The leaching temperature is 60°C to 90°C, and the leaching time is 30min to 150min.
[0023] As a further improvement of the present invention, the acid leaching process further includes:
[0024] The acid leaching residue obtained after suction filtration is washed 1 to 5 times to obtain an acid leaching residue washing liquid and an acid leaching washing residue, and the acid leaching residue washing liquid is returned to prepare the acid solution.
[0025] As a further improvement of the present invention, in the first impurity removal process,
[0026] The mass fraction of the neutralizing precipitant is 10% to 60%;
[0027] Add a neutralizing precipitant and adjust the pH to 4.00-7.00;
[0028] Neutralizing precipitants include, but are not limited to, one or more of the following: calcium hydroxide, calcium carbonate, sodium hydroxide, potassium hydroxide, ammonia water, magnesium carbonate, and sodium carbonate.
[0029] As a further improvement of the present invention, the first impurity removal process further includes:
[0030] The neutralized filter residue obtained after filtration is washed 1 to 5 times to obtain a neutralized filter residue washing liquid and a neutralized washing residue, the neutralized filter residue washing liquid is returned to prepare a neutralization precipitant, and the neutralized washing residue is used to prepare a by-product; wherein the neutralized filter residue contains the valuable metal Al 3+ , Fe 3+ Etc., the by-products include high-strength gypsum, iron oxide and aluminum oxide.
[0031] As a further improvement of the present invention, in the second impurity removal process,
[0032] The mass fraction of the purification precipitant is 10% to 60%;
[0033] Add purification precipitant and adjust pH to 10.00-13.00;
[0034] Purification precipitants include, but are not limited to, one or more of the following: calcium hydroxide, calcium carbonate, sodium hydroxide, potassium hydroxide, ammonia water, magnesium carbonate, and sodium carbonate.
[0035] As a further improvement of the present invention, the second impurity removal process further includes:
[0036] The purified filter residue obtained after filtration is washed 1 to 5 times to obtain a purified filter residue washing liquid and a purified washing residue, the purified filter residue washing liquid is returned to prepare a purified precipitant, and the purified washing residue is returned as a neutralizing precipitant; wherein the purified filter residue contains valuable metal Ca 2+ Mg 2+ wait.
[0037] As a further improvement of the present invention, the enrichment treatment of the purified filtrate to obtain the enriched liquid comprises:
[0038] The purified filtrate is initially enriched by using reverse osmosis technology; wherein the main pressure used by reverse osmosis is 0.1MPa~0.4MPa, the auxiliary pressure is 0.5MPa~4.0MPa, and the temperature is 10℃~30℃.
[0039] The primary enrichment solution is extracted to obtain a deep enrichment solution, wherein the enrichment multiple is 30 to 100 times.
[0040] As a further improvement of the present invention, the lithium precipitation agent includes but is not limited to one or more of the following: sodium carbonate, calcium carbonate, magnesium carbonate, and ammonium carbonate.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] The present invention uses carbonate clay-type lithium ore as raw material and separates the main valuable elements in steps, filling the technical gap in the comprehensive utilization of carbonate clay-type lithium ore; at the same time, the method has the advantages of low cost, easy operation, high efficiency, etc., has significant economic benefits and good application prospects, and comprehensively improves the comprehensive utilization value of carbonate clay-type lithium ore. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 The present invention discloses a flow chart of a method for preparing lithium carbonate from carbonate clay-type lithium ore according to an embodiment of the present invention. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0046] like Figure 1 As shown, the present invention provides a method for preparing lithium carbonate from carbonate clay-type lithium ore, which can achieve effective separation of valuable elements in carbonate clay-type lithium ore and efficient extraction of lithium elements, and specifically includes:
[0047] Step 1, crushing, grinding, screening and roasting the carbonate clay type lithium ore in sequence to obtain roasted clinker;
[0048] Specifically include:
[0049] 1) crushing the carbonate clay type lithium ore to obtain ore material; wherein the particle size of the ore material is 2 mm to 30 mm;
[0050] 2) Grinding the ore to obtain a coarse powder; wherein the grinding time is 10 min to 60 min;
[0051] 3) Screening the coarse powder to obtain an undersize product; wherein the particle size of the undersize product is less than 0.850 mm, and the oversize product is returned to the grinding section for further grinding, and the mass of the undersize product accounts for 60% to 90%;
[0052] 4) roasting the product under the sieve to obtain roasted clinker; wherein the roasting temperature is 300°C to 1500°C.
[0053] Step 2, subjecting the roasted clinker to acid leaching treatment, and then filtering to obtain a leaching solution and an acid leaching residue;
[0054] in,
[0055] The acid used for acid leaching includes, but is not limited to, one or more of the following: sulfuric acid, hydrochloric acid, nitric acid, acetic acid, citric acid, tartaric acid, oxalic acid;
[0056] The mass fraction of the acid solution is 10% to 30%, and the solid-liquid ratio of the roasted clinker to the acid solution is 1:1 to 1:5;
[0057] The leaching temperature is 60℃~90℃, and the leaching time is 30min~150min;
[0058] The acid leaching residue is washed 1 to 5 times to obtain an acid leaching residue washing liquid and an acid leaching washing residue, and the acid leaching residue washing liquid is returned to prepare the acid solution.
[0059] Step 3, adding 10% to 60% by mass of a neutralizing precipitant to the leaching solution, adjusting the pH to 4.00 to 7.00, performing a first impurity removal treatment, and then filtering to obtain a neutralized filtrate and a neutralized filter residue;
[0060] in,
[0061] Neutralizing precipitants include, but are not limited to, one or more of the following: calcium hydroxide, calcium carbonate, sodium hydroxide, potassium hydroxide, ammonia water, magnesium carbonate, sodium carbonate;
[0062] The neutralized filter residue is washed 1 to 5 times to obtain a neutralized filter residue washing liquid and a neutralized washing residue. The neutralized filter residue washing liquid is returned to prepare a neutralization precipitant, and the neutralized washing residue is used to prepare a by-product; wherein the neutralized filter residue contains valuable metal Al 3+ , Fe 3+ Etc., by-products include high-strength gypsum, iron oxide and aluminum oxide.
[0063] Step 4, adding 10% to 60% by mass of a purification precipitant to the neutralized filtrate, adjusting the pH to 10.00 to 13.00, performing a second impurity removal treatment, and then filtering to obtain a purified filtrate and a purified filter residue;
[0064] in,
[0065] Purification precipitants include, but are not limited to, one or more of the following: calcium hydroxide, calcium carbonate, sodium hydroxide, potassium hydroxide, ammonia water, magnesium carbonate, and sodium carbonate.
[0066] The purified filter residue is washed 1 to 5 times to obtain a purified filter residue washing liquid and a purified washing residue, the purified filter residue washing liquid is returned to prepare a purified precipitant, and the purified washing residue is returned as a neutralizing precipitant; wherein the purified filter residue contains valuable metal Ca 2+ Mg 2+ wait.
[0067] Step 5, enriching the purified filtrate to obtain an enriched solution;
[0068] Specifically include:
[0069] 1) The purified filtrate is initially enriched by reverse osmosis technology; wherein the main pressure used in reverse osmosis is 0.1MPa-0.4MPa, the auxiliary pressure is 0.5MPa-4.0MPa, and the temperature is 10°C-30°C.
[0070] 2) Extracting the primary enrichment solution to obtain a deep enrichment solution, wherein the enrichment multiple is 30 to 100 times.
[0071] Step 6, adding a lithium precipitating agent to the deep enrichment solution to obtain high-purity lithium carbonate;
[0072] in,
[0073] Lithium precipitation agents include, but are not limited to, one or more of the following: sodium carbonate, calcium carbonate, magnesium carbonate, and ammonium carbonate.
[0074] Example 1
[0075] The present invention provides a method for preparing lithium carbonate from carbonate clay-type lithium ore, comprising:
[0076] S11, crushing, grinding and screening the carbonate clay-type lithium ore in sequence to obtain a powder with a particle size of less than 0.850 mm; and roasting the powder at 600° C. to obtain a roasted clinker;
[0077] S12, prepare a sulfuric acid solution with a mass fraction of 10%, with a solid-liquid ratio of 1:5, react at 80° C. for 120 min, filter, separate the solid and the liquid, and obtain an leaching solution;
[0078] S13, prepare a calcium carbonate emulsion with a mass fraction of 10%, adjust the pH value of the leaching solution to 6.00, and filter to obtain a neutralized filtrate;
[0079] S14, prepare a sodium carbonate solution with a mass fraction of 30%, adjust the pH value to 13.00, and filter to obtain a purified filtrate;
[0080] S15, the purified filtrate is subjected to reverse osmosis and extraction to obtain a 70-fold enriched solution;
[0081] S16. Adding a sodium carbonate solution with a mass fraction of 30% to the enriched solution to obtain lithium carbonate with a purity of 99.0%, and a lithium recovery rate of more than 98%.
[0082] Example 2
[0083] The present invention provides a method for preparing lithium carbonate from carbonate clay-type lithium ore, comprising:
[0084] S21, crushing, grinding and screening the carbonate clay-type lithium ore in sequence to obtain a powder with a particle size of less than 0.850 mm; and roasting the powder at 1000° C. to obtain a roasted clinker;
[0085] S22, prepare a sulfuric acid solution with a mass fraction of 15%, with a solid-liquid ratio of 1:3, react at 80° C. for 150 min, filter, separate the solid and the liquid, and obtain an leaching solution;
[0086] S23, prepare a calcium carbonate emulsion with a mass fraction of 20%, adjust the pH value of the leaching solution to 5.00, and filter to obtain a neutralized filtrate;
[0087] S24, prepare a sodium carbonate solution with a mass fraction of 30%, adjust the pH value to 10.00, and filter to obtain a purified filtrate;
[0088] S25, the purified filtrate is subjected to reverse osmosis and extraction to obtain a 70-fold enriched solution;
[0089] S26. Adding a sodium carbonate solution with a mass fraction of 30% to the enriched solution to obtain lithium carbonate with a purity greater than 99.5%, and a lithium recovery rate greater than 99%.
[0090] The advantages of the present invention are:
[0091] The process flow of the present invention fills the gap in the comprehensive utilization of carbonate clay-type lithium ore, can realize the efficient separation of various valuable elements such as aluminum, iron, calcium, magnesium and the like and the efficient and high-purity extraction of lithium element, and the tailings can be directly returned to the previous process section, effectively solving the problems of low grade of lithium ore, high energy consumption and low recovery rate, improving the comprehensive utilization rate of carbonate clay-type lithium ore, and providing a technical basis for the development and utilization of lithium resources.
[0092] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing lithium carbonate from carbonate clay-type lithium ore, characterized in that: include: The carbonate clay type lithium ore is crushed, ground, screened and roasted in sequence to obtain roasted clinker; The roasted clinker is subjected to acid leaching treatment, and then filtered to obtain a leaching solution; Adding a neutralizing precipitant to the leaching solution for a first impurity removal treatment, and then filtering to obtain a neutralized filtrate; Adding a purification precipitant to the neutralized filtrate to perform a second impurity removal treatment, and then filtering to obtain a purified filtrate; Performing enrichment treatment on the purified filtrate to obtain an enriched liquid; A lithium precipitating agent is added to the enriched solution to obtain lithium carbonate.
2. The method according to claim 1, characterized in that The method of crushing, grinding, screening and roasting the carbonate clay type lithium ore in sequence to obtain roasted clinker comprises: Crushing the carbonate clay type lithium ore to obtain ore material; wherein the particle size of the ore material is 2 mm to 30 mm; Grinding the ore to obtain a coarse powder; wherein the grinding time is 10 minutes to 60 minutes; The coarse powder is screened to obtain the undersize product; wherein the particle size of the undersize product is less than 0.850 mm, and the oversize product is returned to the grinding section for further grinding, and the mass of the undersize product accounts for 60% to 90%; The product under the sieve is roasted to obtain roasted clinker; wherein the roasting temperature is 300°C to 1500°C.
3. The method according to claim 1, characterized in that In the acid leaching process, The acid used includes, but is not limited to, one or more of the following: sulfuric acid, hydrochloric acid, nitric acid, acetic acid, citric acid, tartaric acid, oxalic acid; The mass fraction of the acid solution is 10% to 30%, and the solid-liquid ratio of the roasted clinker to the acid solution is 1:1 to 1:5; The leaching temperature is 60°C to 90°C, and the leaching time is 30min to 150min.
4. The method according to claim 3, characterized in that The pickling process also includes: The acid leaching residue obtained after suction filtration is washed 1 to 5 times to obtain an acid leaching residue washing liquid and an acid leaching washing residue, and the acid leaching residue washing liquid is returned to prepare the acid solution.
5. The method according to claim 1, characterized in that In the first impurity removal process, The mass fraction of the neutralizing precipitant is 10% to 60%; Add a neutralizing precipitant and adjust the pH to 4.00-7.00; Neutralizing precipitants include, but are not limited to, one or more of the following: calcium hydroxide, calcium carbonate, sodium hydroxide, potassium hydroxide, ammonia water, magnesium carbonate, and sodium carbonate.
6. The method according to claim 1, characterized in that The first impurity removal process also includes: The neutralized filter residue obtained after filtration is washed 1 to 5 times to obtain a neutralized filter residue washing liquid and a neutralized washing residue, the neutralized filter residue washing liquid is returned to prepare a neutralization precipitant, and the neutralized washing residue is used to prepare a by-product; wherein the neutralized filter residue contains the valuable metal Al 3+ , Fe 3+ , the by-products include high-strength gypsum, iron oxide and aluminum oxide.
7. The method according to claim 1, characterized in that In the second impurity removal process, The mass fraction of the purification precipitant is 10% to 60%; Add purification precipitant and adjust pH to 10.00-13.00; Purification precipitants include, but are not limited to, one or more of the following: calcium hydroxide, calcium carbonate, sodium hydroxide, potassium hydroxide, ammonia water, magnesium carbonate, and sodium carbonate.
8. The method according to claim 7, characterized in that The second impurity removal process also includes: The purified filter residue obtained after filtration is washed 1 to 5 times to obtain a purified filter residue washing liquid and a purified washing residue, the purified filter residue washing liquid is returned to prepare a purified precipitant, and the purified washing residue is returned as a neutralizing precipitant; wherein the purified filter residue contains valuable metal Ca 2+ Mg 2+ .
9. The method according to claim 1, characterized in that The enrichment treatment of the purified filtrate to obtain an enriched solution comprises: The purified filtrate is initially enriched by using reverse osmosis technology; wherein the main pressure used by reverse osmosis is 0.1MPa~0.4MPa, the auxiliary pressure is 0.5MPa~4.0MPa, and the temperature is 10℃~30℃. The primary enrichment solution is extracted to obtain a deep enrichment solution, wherein the enrichment multiple is 30 to 100 times.
10. The method according to claim 1, characterized in that The lithium precipitation agent includes but is not limited to one or more of the following: sodium carbonate, calcium carbonate, magnesium carbonate, and ammonium carbonate.
Citation Information
Cited By
Grinding and leaching integrated gradient lithium extraction method for clay type lithium ore
CN120006112A