Hydrogenation method for purifying industrial-grade lithium carbonate and process for purifying industrial-grade lithium carbonate by adopting hydrogenation method

By using supercritical carbon dioxide fluid and pressure reduction technology in the lithium carbonate purification process, the problem of CO2 gas dissolution rate limitation is solved, the conversion rate and purity of lithium carbonate are improved, and efficient lithium carbonate purification is achieved.

CN118724031APending Publication Date: 2024-10-01YONGZHOU HAOLI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410881438.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing lithium carbonate purification process, the conversion rate and speed of Li2CO3 into LiHCO3 are limited by the dissolution rate of CO2 gas in water, resulting in a long conversion time and reducing the conversion rate and yield of lithium carbonate.

Method used

The supercritical carbon dioxide fluid is stirred and depressurized in the hydrogenation reactor to control the pressure and temperature in the hydrogenation reactor, shorten the hydrogenation time, and improve the efficiency of converting Li2CO3 into LiHCO3.

Benefits of technology

The conversion rate during the hydrogenation process and the yield and purity of high-purity lithium carbonate are significantly improved, the hydrogenation time is shortened, and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724031A_ABST
    Figure CN118724031A_ABST
Patent Text Reader

Abstract

The invention discloses a hydrogenation method for purifying industrial-grade lithium carbonate and a process for purifying the industrial-grade lithium carbonate by adopting the method, and the hydrogenation method comprises the following steps: 1) inputting the industrial-grade lithium carbonate and pure water into a hydrogenation reaction kettle, stirring and mixing to prepare crude lithium carbonate slurry; 2) introducing supercritical carbon dioxide fluid, controlling the pressure in the hydrogenation reaction kettle to be 25-30MPa and the temperature to be 25-30 DEG C, and stirring for 2-3 minutes; and reducing the pressure in the hydrogenation reaction kettle to 5-6 MPa at the pressure reduction speed of 10-15 MPa / min, reacting for 10-15 minutes at the temperature of 32-35 DEG C, filtering, and collecting the hydrogenated liquid obtained by filtering. In the hydrogenation process, the supercritical carbon dioxide fluid is firstly introduced, and then the pressure is reduced, so that the conversion rate of converting Li2CO3 into LiHCO3 in the hydrogenation process is improved, the hydrogenation time is shortened, the hydrogenation efficiency is improved, and the hydrogenation cost is reduced; by adopting the hydrogenation method to purify the industrial-grade lithium carbonate, the yield, the purity and the purification efficiency of the lithium carbonate can be improved, and the purification cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium carbonate purification, and in particular to a hydrogenation method for purifying industrial-grade lithium carbonate and a process for purifying industrial-grade lithium carbonate by using the method. Background Art

[0002] Lithium carbonate is the main raw material for the preparation of other high-purity lithium alloys and lithium compounds. It is the most widely used lithium compound in the lithium salt industry and has been widely used in aluminum smelting, glass, ceramics, battery, pharmaceutical and electronics industries.

[0003] The existing lithium carbonate is mainly produced by using the lithium-containing liquid after extracting barium chloride from salt lake brine, removing calcium and magnesium ions with soda ash, acidifying with hydrochloric acid, and then reacting with soda ash. However, due to the limitations of production technology and salt lake brine itself, most of the primary products are industrial-grade lithium carbonate with low purity and low added value. It is necessary to purify the industrial-grade lithium carbonate to prepare high-purity, high-value-added lithium carbonate.

[0004] Industrial-grade lithium carbonate can be purified by electrolysis, hydrogenation precipitation, hydrogenation decomposition, etc. The hydrogenation decomposition method includes two processes: hydrogenation and thermal analysis. The hydrogenation process is to mix industrial-grade Li2CO3 and deionized water in a certain proportion into a slurry, and introduce CO2 gas during stirring to convert the slightly soluble Li2CO3 in water into LiHCO3 with much greater solubility. Most other impurities cannot be hydrogenated, and insoluble carbonates can be removed by filtration to obtain hydrogenated liquid. The thermal analysis process is to heat the filtrate after removing impurities, stir at a constant temperature to remove CO2 gas, cool it down, filter it, and obtain a precipitate. After drying, a high-purity Li2CO3 product is obtained.

[0005] CN202310313790.8 discloses a purification process for purifying industrial-grade lithium carbonate to prepare battery-grade lithium carbonate, which adopts the hydrogenation decomposition method to purify crude lithium carbonate. The steps are as follows: adding crude lithium carbonate and deionized water in a weight ratio of 1:20 into a carbonization dissolution chamber in a re-purification reaction device, stirring evenly to obtain a mixed slurry, and introducing carbon dioxide from the inner bottom of the carbonization dissolution chamber through a carbon dioxide pipeline at a flow rate of 8-10L / min and an introduction time of 40-60min. Then, after the mixed slurry is filtered, the filtrate is transferred to a crystallization chamber, the temperature of the crystallization chamber is set to 85-95°C, the stirring speed is 300-360r / min, the reaction is 70-90min, the temperature of the crystallization chamber is lowered to room temperature, the filter is suction filtered, the filter cake is rinsed with purified water, drained, transferred to a drying oven at a temperature of 75-85°C, and dried for 10-14h to obtain battery-grade lithium carbonate.

[0006] In the process of purifying industrial-grade lithium carbonate using this process, the conversion rate and speed of Li2CO3 into highly soluble LiHCO3 are related to the dissolution of CO2 gas. CO2 gas needs to be dissolved before reacting with Li2CO3 to convert into LiHCO3 when it is introduced into the slurry containing water and Li2CO3. However, due to the limited dissolution rate of CO2 gas in water, it cannot dissolve quickly and fully contact the Li2CO3 particles in the slurry, resulting in a long conversion time required for Li2CO3 to LiHCO3, which greatly reduces the conversion rate and yield of lithium carbonate. Summary of the invention

[0007] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a hydrogenation method for purifying industrial-grade lithium carbonate and a process for purifying industrial-grade lithium carbonate using the method, wherein the method can improve the conversion rate in the hydrogenation process and the yield and purity of high-purity lithium carbonate.

[0008] The technical solution adopted by the present invention to solve the technical problem is: a hydrogenation method for purifying industrial-grade lithium carbonate, comprising the following steps:

[0009] 1) introducing industrial-grade lithium carbonate and pure water into a hydrogenation reactor, stirring and mixing to prepare a crude lithium carbonate slurry;

[0010] 2) introducing supercritical carbon dioxide fluid, controlling the pressure in the hydrogenation reaction kettle to be 25-30 MPa, the temperature to be 25-30° C., and stirring for 2-3 min; then reducing the pressure in the hydrogenation reaction kettle to 5-6 MPa at a pressure reduction rate of 10-15 MPa / min, reacting at a temperature of 32-35° C. for 10-15 min, filtering, and collecting the hydrogenated liquid obtained by filtration.

[0011] Furthermore, in step 1), the solid-to-liquid ratio of industrial-grade lithium carbonate to pure water is 1:20-30.

[0012] Preferably, supercritical carbon dioxide fluid is introduced in step 2), the pressure in the hydrogenation reactor is controlled to be 25 MPa, the temperature is controlled to be 25° C., and stirring is performed for 2 minutes.

[0013] Preferably, in step 2), the pressure reduction rate in the hydrogenation reaction kettle is 10 MPa / min, and the pressure in the hydrogenation reaction kettle is reduced to 5 MPa, and the reaction is carried out at a temperature of 35° C. for 10 minutes.

[0014] The present invention also provides a process for purifying industrial-grade lithium carbonate using the hydrogenation method as described above, comprising the following steps:

[0015] a) Thermal analysis: placing the obtained hydrogenated liquid in a thermal decomposition reactor, stirring, introducing steam, heating to 80-90°C while stirring, and then keeping the temperature for 40-50 minutes to obtain lithium carbonate slurry; the collected carbon dioxide gas can be pressurized to 25-30MPa to form a supercritical carbon dioxide fluid for recycling;

[0016] b) Centrifugal dehydration: transferring the lithium carbonate slurry into a centrifuge, starting the centrifuge to dehydrate, and obtaining lithium carbonate mother liquor and wet lithium carbonate;

[0017] c) Drying and crushing: The wet lithium carbonate is transferred into a dryer for drying, and then the dried lithium carbonate is transferred into a crusher for crushing until the particle size D50 reaches 3 μm-8 μm;

[0018] d) Testing and packaging: Check whether the content of magnetic substances in the crushed lithium carbonate is ≤500ppb. If the content of magnetic substances is >500ppb, demagnetization treatment is performed; if the content of magnetic substances is ≤500ppb, high-purity lithium carbonate with a purity of ≥99.9% is directly packaged.

[0019] Furthermore, the moisture content in the wet lithium carbonate is 12%-14%.

[0020] Furthermore, the lithium carbonate mother liquor is sent to a circulation pool for cooling, and then circulated back to the hydrogenation reactor to prepare a crude lithium carbonate slurry.

[0021] Furthermore, when the lithium carbonate mother liquor is recycled to prepare crude lithium carbonate slurry, the volume ratio of the lithium carbonate mother liquor to pure water is 0.5:1.

[0022] Furthermore, in step c), the drying temperature is 90-100° C. and the drying time is 60-90 min.

[0023] The beneficial effects of a hydrogenation method for purifying industrial-grade lithium carbonate and a process for purifying industrial-grade lithium carbonate using the method are as follows:

[0024] (1) The hydrogenation method of the present invention is simple. In the hydrogenation process, a supercritical carbon dioxide fluid is first introduced and then the pressure is reduced, which overcomes the technical barrier of directly introducing carbon dioxide gas in the conventional method. The method can not only greatly improve the conversion rate of Li2CO3 to LiHCO3 in the hydrogenation process, but also effectively shorten the hydrogenation time, so that the entire hydrogenation time is shortened from 30min-120min in the conventional method to less than 20min, thereby greatly improving the hydrogenation efficiency and reducing the hydrogenation cost.

[0025] (2) The process of purifying industrial-grade lithium carbonate using the hydrogenation method of the present invention can not only greatly improve the yield and purity of lithium carbonate, but also greatly shorten the purification time, improve the purification efficiency, and reduce the purification cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 — is a flow chart of a hydrogenation method for purifying industrial-grade lithium carbonate and a process for purifying industrial-grade lithium carbonate using the method according to the present invention. DETAILED DESCRIPTION

[0027] The present invention is further described below in conjunction with the accompanying drawings and examples, but these specific implementation schemes do not limit the protection scope of the present invention in any way.

[0028] Example 1

[0029] A hydrogenation method for purifying industrial grade lithium carbonate, see Figure 1 , including the following steps:

[0030] 1) Weigh 2.0 kg of industrial-grade lithium carbonate with a purity of 99.2%, input the industrial-grade lithium carbonate and pure water into a hydrogenation reactor at a solid-to-liquid ratio of 1:30, and stir and mix to prepare a crude lithium carbonate slurry;

[0031] 2) Supercritical carbon dioxide fluid is introduced, the pressure in the hydrogenation reactor is controlled to be 25MPa, the temperature is 25°C, and stirring is performed for 2min; the pressure in the hydrogenation reactor is reduced to 6MPa at a depressurization rate of 15MPa / min, the reaction is performed for 10min at a temperature of 35°C, and the hydrogenated liquid obtained by filtration is collected. The hydrogenation time is the reaction time after the introduction of carbon dioxide, and the starting time is the timing started when the supercritical carbon dioxide fluid is introduced, and the end time is the critical time point after the pressure is reduced to the set pressure (6Mpa in the present embodiment) and the reaction set time (10min in the present embodiment), and the entire hydrogenation time is about 13min.

[0032] Example 2

[0033] A hydrogenation method for purifying industrial-grade lithium carbonate comprises the following steps:

[0034] 1) Weigh 2.0 kg of industrial-grade lithium carbonate with a purity of 99.2%, input the industrial-grade lithium carbonate and pure water into a hydrogenation reactor at a solid-to-liquid ratio of 1:25, and stir and mix to prepare a crude lithium carbonate slurry;

[0035] 2) Supercritical carbon dioxide fluid was introduced, the pressure in the hydrogenation reactor was controlled to be 25 MPa, the temperature was 30°C, and the mixture was stirred for 2 min; the pressure in the hydrogenation reactor was then reduced to 5 MPa at a pressure reduction rate of 10 MPa / min, the mixture was reacted at a temperature of 35°C for 10 min, and the hydrogenated liquid was filtered and collected. The entire hydrogenation time was about 14 min.

[0036] Example 3

[0037] A hydrogenation method for purifying industrial-grade lithium carbonate comprises the following steps:

[0038] 1) Weigh 2.0 kg of industrial-grade lithium carbonate with a purity of 99.2%, input the industrial-grade lithium carbonate and pure water into a hydrogenation reactor at a solid-to-liquid ratio of 1:20, and stir and mix to prepare a crude lithium carbonate slurry;

[0039] 2) Supercritical carbon dioxide fluid was introduced, the pressure in the hydrogenation reactor was controlled to be 30 MPa, the temperature was 30°C, and stirring was performed for 3 minutes; then the pressure in the hydrogenation reactor was reduced to 5 MPa at a pressure reduction rate of 10 MPa / min, and the reaction was carried out at a temperature of 32°C for 15 minutes, and the filtered hydrogenated liquid was collected. The entire hydrogenation time was about 20 minutes.

[0040] Example 4

[0041] A method for purifying industrial-grade lithium carbonate, wherein the hydrogenated liquid prepared by the hydrogenation method of Example 1 is used to purify industrial-grade lithium carbonate, see Figure 1 , specifically including the following steps:

[0042] a) Thermal analysis: placing the obtained hydrogenated liquid in a thermal decomposition reactor, stirring, introducing steam, heating to 90° C. while stirring, and then keeping the temperature for 40 minutes to obtain lithium carbonate slurry; the lithium carbonate mother liquor is sent to a circulation pool for cooling, and then recycled back to the hydrogenation reactor to prepare the next batch of crude lithium carbonate slurry. When the lithium carbonate mother liquor is recycled to prepare the crude lithium carbonate slurry, the volume ratio of the lithium carbonate mother liquor to pure water is 0.5:1; the collected carbon dioxide gas can be pressurized to form a supercritical carbon dioxide fluid for circulation in the hydrogenation process of the next batch of industrial-grade lithium carbonate;

[0043] b) centrifugal dehydration: transferring the lithium carbonate slurry into a centrifuge, starting the centrifuge for dehydration, and obtaining a lithium carbonate mother liquor and wet lithium carbonate, wherein the water content of the wet lithium carbonate is 12%-14%;

[0044] c) Drying and crushing: The wet lithium carbonate is transferred into a dryer and dried at 100° C. for 60 min, and then the dried lithium carbonate is transferred into a crusher and crushed to a particle size D50 of 3 μm-8 μm;

[0045] d) Testing and packaging: The content of magnetic substances in the crushed lithium carbonate is tested to be ≤500ppb, and then directly packaged to obtain high-purity lithium carbonate with a purity of 99.95%.

[0046] Example 5

[0047] The difference between this embodiment and embodiment 4 is that the hydrogenated liquid prepared by the hydrogenation method of embodiment 2 is used to purify industrial-grade lithium carbonate.

[0048] Example 6

[0049] The difference between this embodiment and embodiment 4 is that the hydrogenated liquid prepared by the hydrogenation method of embodiment 3 is used to purify industrial-grade lithium carbonate.

[0050] Comparative Example 1

[0051] This comparative example adopts a traditional hydrogenation method (such as CN202310313790.8) to carry out a hydrogenation reaction, which specifically includes the following steps:

[0052] 1) Weigh 2.0 kg of industrial-grade lithium carbonate with a purity of 99.2%, input the industrial-grade lithium carbonate and pure water into a hydrogenation reactor at a solid-to-liquid ratio of 1:20, and stir and mix to prepare a crude lithium carbonate slurry;

[0053] 2) introducing carbon dioxide gas into a hydrogenation reactor at a pressure of 6 MPa, reacting at a temperature of 32° C. and a pressure of 6 MPa for 60 min, filtering, collecting the hydrogenated liquid obtained by filtration, and purifying industrial-grade lithium carbonate using the hydrogenated liquid and the thermal analysis and subsequent operation methods in Reference Example 1.

[0054] Comparative Example 2

[0055] The difference between this comparative example and comparative example 1 is that the reaction time is 13 minutes, and the hydrogenation liquid prepared in comparative example 2 is used and the thermal analysis and subsequent operation methods in reference example 1 are used to purify industrial-grade lithium carbonate.

[0056] The present invention measures the conversion rate of lithium carbonate in the hydrogenated liquid obtained by the hydrogenation method of Examples 1-3 and Comparative Examples 1-2, and measures the yield and purity of high-purity lithium carbonate obtained by purification of Examples 4-6 and Comparative Examples 1-2.

[0057] Among them, the mass of lithium carbonate is determined by acid-base titration, the conversion rate of lithium carbonate in hydrogenated solution (%) = (the mass of lithium carbonate in industrial-grade lithium carbonate - the mass of lithium carbonate in hydrogenated solution) / the mass of lithium carbonate in industrial-grade lithium carbonate, the yield of high-purity lithium carbonate (%) = the mass of lithium carbonate in high-purity lithium carbonate / the mass of lithium carbonate in industrial-grade lithium carbonate, and the purity (%) = the mass of lithium carbonate in high-purity lithium carbonate / the mass of high-purity lithium carbonate.

[0058] The test results are shown in Table 1-2:

[0059] Table 1 The mass of lithium carbonate in the corresponding samples in Examples 1-6 and Comparative Examples 1-2

[0060]

[0061] Table 2 Corresponding conversion rate, yield and purity in Examples 1-6 and Comparative Examples 1-2

[0062] Conversion rate / % Yield / % purity / % Hydrogenation time / min Example 1 98.9 / / 13 Example 2 98.9 / / 14 Example 3 99 / / 20 Comparative Example 1 90 90.0 99.5 60 Comparative Example 2 85.1 85.0 99.3 13 Example 4 98.9 98.8 99.95 13 Example 5 98.9 98.8 99.95 14 Example 6 99 98.9 99.97 20

[0063] As can be seen from the above table, the hydrogenation time of the hydrogenation method corresponding to Examples 1-3 is within 20 minutes, at least 13 minutes, and the conversion rate of lithium carbonate in the hydrogenation solution into lithium bicarbonate is as high as 98.8%, and the yield of high-purity lithium carbonate (corresponding to Examples 4, 5 and 6, respectively) prepared by the hydrogenation method reaches 98.8%, and the purity reaches 99.95%;

[0064] However, when the conventional carbon dioxide gas was introduced and reacted for 60 minutes in Comparative Example 1, the corresponding conversion rate was 90%, and the conventional carbon dioxide gas was introduced and reacted for the same hydrogenation time as in Example 1, and the corresponding conversion rate was only 85.1%. The yield and purity of the high-purity lithium carbonate prepared in Comparative Examples 1 and 2 were significantly lower than those in Example 4. This may be because the conversion rate of lithium carbonate in the hydrogenation reaction process in Comparative Examples 1 and 2 was significantly lower than that in Example 1. The mechanism is as follows:

[0065] The principle of hydrogenation reaction is: Li2CO3+CO2+H2O=2LiHCO3. During the reaction, carbon dioxide gas needs to be dissolved in water to form H + , H + It then reacts with Li2CO3 to form LiHCO3 with high solubility. Since Comparative Examples 1 and 2 use the traditional method of introducing CO2 gas to carry out the hydrogenation reaction, the dissolution rate of CO2 gas in water is limited, and it cannot dissolve quickly and fully contact with the Li2CO3 particles in the slurry, resulting in a long conversion time required for Li2CO3 to be converted into LiHCO3, resulting in a low conversion rate of lithium carbonate during the hydrogenation reaction, which greatly reduces the purity and yield of the purified lithium carbonate.

[0066] In this embodiment 1-3, a method of first introducing a supercritical carbon dioxide fluid and then reducing the pressure to form carbon dioxide gas for hydrogenation reaction is adopted. After the supercritical carbon dioxide fluid is introduced into the hydrogenation reaction kettle, it can be evenly dispersed in the crude lithium carbonate slurry under stirring, and the supercritical carbon dioxide fluid is evenly dispersed around each lithium carbonate particle and in the water.

[0067] Then, by reducing the pressure, the supercritical carbon dioxide fluid is gradually converted into carbon dioxide gas, so that carbon dioxide gas is distributed around each lithium carbonate particle and in the water, which not only increases the contact area between carbon dioxide gas and water and promotes the dissolution rate of carbon dioxide in water, but also each lithium carbonate particle can be wrapped by the hydrogen ion solution formed by dissolving carbon dioxide gas, increasing the contact area between each lithium carbonate particle and the hydrogen ion solution, thereby accelerating the formation of lithium bicarbonate, effectively shortening the time of the hydrogenation reaction, and increasing the conversion rate of lithium carbonate to lithium bicarbonate during the hydrogenation reaction. Ultimately, the yield of high-purity lithium carbonate obtained by purifying industrial-grade lithium carbonate using the hydrogenation method is as high as 98.8%, and the purity is as high as 99.95%.

[0068] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A hydrogenation method for purifying industrial-grade lithium carbonate, characterized in that: The following steps are involved: 1) introducing industrial-grade lithium carbonate and pure water into a hydrogenation reactor, stirring and mixing to prepare a crude lithium carbonate slurry; 2) introducing supercritical carbon dioxide fluid, controlling the pressure in the hydrogenation reaction kettle to be 25-30 MPa, the temperature to be 25-30° C., and stirring for 2-3 min; then reducing the pressure in the hydrogenation reaction kettle to 5-6 MPa at a pressure reduction rate of 10-15 MPa / min, reacting at a temperature of 32-35° C. for 10-15 min, filtering, and collecting the hydrogenated liquid obtained by filtration.

2. A hydrogenation method for purifying industrial grade lithium carbonate as claimed in claim 1, characterized in that: In the step 1), the solid-to-liquid ratio of industrial-grade lithium carbonate to pure water is 1:20-30.

3. A hydrogenation method for purifying industrial grade lithium carbonate as claimed in claim 1, characterized in that: In the step 2), supercritical carbon dioxide fluid is introduced, the pressure in the hydrogenation reactor is controlled to be 25 MPa, the temperature is 25° C., and stirring is performed for 2 minutes.

4. A hydrogenation method for purifying industrial grade lithium carbonate as claimed in claim 1, characterized in that: In the step 2), the pressure reduction rate in the hydrogenation reaction kettle is 10 MPa / min, and the pressure in the hydrogenation reaction kettle is reduced to 5 MPa, and the reaction is carried out at a temperature of 35° C. for 10 minutes.

5. A process for purifying industrial grade lithium carbonate using the hydrogenation method according to any one of claims 1 to 4, characterized in that: The following steps are involved: a) Thermal analysis: placing the obtained hydrogenated liquid in a thermal decomposition reactor, stirring, introducing steam, heating to 80-90° C. while stirring, and then keeping the temperature for 40-50 min to obtain lithium carbonate slurry; b) Centrifugal dehydration: transferring the lithium carbonate slurry into a centrifuge, starting the centrifuge to dehydrate, and obtaining lithium carbonate mother liquor and wet lithium carbonate; c) Drying and crushing: The wet lithium carbonate is transferred into a dryer for drying, and then the dried lithium carbonate is transferred into a crusher for crushing until the particle size D50 reaches 3 μm-8 μm; d) Testing and packaging: Check whether the content of magnetic substances in the crushed lithium carbonate is ≤500ppb. If the content of magnetic substances is >500ppb, demagnetization treatment is performed; if the content of magnetic substances is ≤500ppb, high-purity lithium carbonate with a purity of ≥99.9% is directly packaged.

6. A process for purifying industrial grade lithium carbonate by hydrogenation as claimed in claim 5, characterized in that: The moisture content in the wet lithium carbonate is 12%-14%.

7. A process for purifying industrial grade lithium carbonate by hydrogenation as claimed in claim 5, characterized in that: The lithium carbonate mother liquor is sent to a circulation pool for cooling and then circulated back to the hydrogenation reactor to prepare a crude lithium carbonate slurry.

8. A process for purifying industrial grade lithium carbonate by hydrogenation as claimed in claim 7, characterized in that: When the lithium carbonate mother liquor is recycled to prepare crude lithium carbonate slurry, the volume ratio of the lithium carbonate mother liquor to pure water is 0.5:

1.

9. A process for purifying industrial grade lithium carbonate by hydrogenation as claimed in claim 5, characterized in that: The drying temperature in step c) is 90-100° C. and the drying time is 60-90 min.

Citation Information

Cited By

  • Preparation method of high-purity battery-grade lithium fluoride

    CN119683660A

  • Preparation method of battery-grade lithium fluoride

    CN119683661A