Preparation method of molybdenum disulfide with micro-nano structure, hydrophobic anti-icing coating based on molybdenum disulfide as well as preparation method and application of hydrophobic anti-icing coating

Micro-nano structure molybdenum disulfide is prepared through the oxidation and hydrothermal reaction of commercial molybdenum dioxide, and combined with modifiers to form a hydrophobic anti-icing coating based on molybdenum disulfide, which solves the problem of insufficient performance of existing MoS2 anti-icing coatings and achieves It achieves high-efficiency, low-cost anti-icing effect and meets environmental protection requirements.

CN118724065APending Publication Date: 2024-10-01GUANGDONG UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410963808.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing MoS2 anti-icing coating has poor hydrophobicity and insignificant photothermal effect, resulting in poor anti-icing performance. The preparation process from natural molybdenite to high-purity MoS2 is complex and costly, limiting its application value.

Method used

Micro-nano structure molybdenum disulfide was prepared using commercial molybdenum dioxide through hydrogen peroxide oxidation and hydrothermal reaction, and was modified with γ-aminopropyltriethoxysilane and combined with fluorine-free polydimethylsiloxane to form Hydrophobic anti-icing coating based on molybdenum disulfide significantly improves its hydrophobic performance and photothermal effect.

Benefits of technology

The preparation of micro-nano structure molybdenum disulfide at low cost and low energy consumption has been achieved, which significantly improves its hydrophobic properties and photothermal effect, prolongs the freezing time of water and accelerates the melting of frost, improves the anti-icing effect, and conforms to the concept of green environmental protection .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724065A_ABST
    Figure CN118724065A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of composite functional materials, in particular to a preparation method of molybdenum disulfide with a micro-nano structure, a hydrophobic anti-icing coating based on molybdenum disulfide and a preparation method and application of the hydrophobic anti-icing coating. In addition, the sulfur source is added again after the sulfur in the molybdenum disulfide is removed through the oxidation reaction, the size of the molybdenum disulfide can be greatly reduced, the nanoscale size is achieved, and therefore a good new way can be provided for follow-up efficient utilization of molybdenite. Moreover, the preparation method of the molybdenum disulfide with the micro-nano structure is simple in whole process, simple and convenient, low in preparation cost and high in preparation efficiency, nanocrystallization of large-size molybdenum disulfide is achieved, and the photothermal effect is remarkably improved. And the prepared hydrophobic anti-icing coating and coating based on molybdenum disulfide not only have a remarkable photothermal effect and can effectively prolong the icing time of water, but also can accelerate the melting process of frost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite functional materials, and in particular to a method for preparing micro-nanostructured molybdenum disulfide, a hydrophobic anti-icing coating based on molybdenum disulfide, and a preparation method and application thereof. Background Art

[0002] In nature, icing causes significant damage to infrastructure such as buildings, aviation, transportation, and power transmission, and even threatens human life and property safety. Although a variety of physical and chemical anti-icing technologies have been proposed, it is still difficult to completely avoid the phenomenon of water molecules spontaneously forming ice crystals under low temperature and high humidity conditions. Therefore, studying how to delay icing, effectively prevent icing and de-icing is also one of the important topics in the field of anti-icing technology.

[0003] Photothermal composite hydrophobic materials have become a hot topic in anti-icing technology research due to their excellent advantages in inhibiting ice nucleus growth, delaying ice formation time, and natural rapid deicing characteristics. For example, the invention patent application with patent publication number CN112724830A discloses a graphene-added anti-fouling and anti-icing water-based coating, which combines the characteristics of super-hydrophobic materials and near-infrared photothermal materials, effectively prolongs the freezing time of water droplets on the coating surface, and improves the anti-icing effect. However, due to the high cost of graphene, it has certain limitations in industrial application and large-scale promotion.

[0004] Molybdenum disulfide (MoS2) is a two-dimensional black material with abundant resources and low cost, and has broad application prospects in my country. As a typical layered stacked two-dimensional material, its particle size and number of layers will affect the wettability of the material surface, making it exhibit hydrophilic, hydrophobic or amphiphilic properties. In addition, MoS2 is the main component of molybdenite, and natural molybdenite is one of the six major advantageous minerals in my country with abundant resources. Despite this, the preparation process from natural molybdenite to high-purity MoS2 is still complicated and costly, and natural molybdenite has high crystallinity, coarse particle size, and is mostly in the form of agglomerates with poor performance. How to effectively develop and utilize large blocks of MoS2 has become the key to improving its application value.

[0005] The invention patent application with patent publication number CN113773732A proposes a MoS2 anti-icing coating, the coating prepared by which can delay the crystallization process of droplets and reduce the crystallization temperature, thereby improving the power generation efficiency and service life of the wind turbine. In addition, the invention patent application with patent publication number CN106867332 A discloses a MoS2 anti-icing coating for viaducts, its preparation method and application, which can effectively prevent ice from forming at the overflow port of the viaduct and reduce the risk of forming large ice blocks. However, these prior arts do not involve the hydrophobic modification of MoS2 and its photothermal effect in the field of anti-icing. Therefore, the MoS2 anti-icing coating of the prior art has poor hydrophobicity, insignificant photothermal effect, and poor anti-icing performance. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the first object of the present invention is to provide a method for preparing micro-nanostructured molybdenum disulfide, which has a simple preparation process and low production cost.

[0007] In order to overcome the shortcomings of the prior art, the second purpose of the present invention is to provide an application of molybdenite to prepare micro-nanostructured molybdenum disulfide, which is a new way to efficiently utilize molybdenite resources.

[0008] The third object of the present invention is to provide a preparation method of a hydrophobic anti-icing coating based on molybdenum disulfide. The preparation method is simple, the conditions are mild, and it is environmentally friendly. The prepared hydrophobic anti-icing coating based on molybdenum disulfide has good hydrophobic properties and a significant photothermal effect. It can effectively prolong the freezing time of water and accelerate the melting process of frost.

[0009] The fourth object of the present invention is to provide a hydrophobic anti-icing coating based on molybdenum disulfide, which has good hydrophobic properties and significant photothermal effect, can effectively prolong the freezing time of water, and can accelerate the melting process of frost.

[0010] A fifth object of the present invention is to provide an application of a hydrophobic anti-icing coating based on molybdenum disulfide.

[0011] In order to achieve the first object of the above invention, the technical solution adopted by the present invention is as follows:

[0012] The invention provides a method for preparing micro-nano structured molybdenum disulfide, comprising the following steps: adding commercial molybdenum dioxide into a hydrogen peroxide solution for oxidation reaction, then adding thiourea, placing the solution in a hydrothermal reactor for hydrothermal reaction, and then washing and drying to obtain the micro-nano structured molybdenum disulfide.

[0013] The preparation method of the micro-nano structured molybdenum disulfide of the present invention is to use hydrogen peroxide to perform oxidation pretreatment on commercial large-sized molybdenum disulfide particles, add thiourea as a new sulfur source, and convert the commercial molybdenum disulfide into molybdenum disulfide with a special morphology through a hydrothermal synthesis method, and the average size of the prepared molybdenum disulfide is about 300nm. Among them, the commercial molybdenum disulfide is added to a hydrogen peroxide solution for oxidation reaction, and the sulfur is removed in the form of hydrogen sulfide. At this time, there is only a Mo source in the system, and thiourea is subsequently added as a sulfur source to resynthesize molybdenum disulfide, that is, the preparation method can change the morphology of commercial molybdenum disulfide through simple processing steps, and after the sulfur of molybdenum disulfide is removed by oxidation reaction first and then the sulfur source is re-added, the size of molybdenum disulfide can be greatly reduced and reach the nanometer size, so it can provide a good way for the subsequent use of molybdenite. In addition, the whole process of the preparation method of the micro-nano structured molybdenum disulfide is simple, the preparation cost is low, and the preparation efficiency is high, and the nanometerization of large-sized molybdenum disulfide is realized.

[0014] Among them, using hydrogen peroxide as an oxidant also has the advantages of low cost and being green and environmentally friendly.

[0015] Furthermore, the size of the commercial molybdenum dioxide is 5 μm to 30 μm; and / or

[0016] The mass concentration of the hydrogen peroxide solution is 8% to 12%; and / or

[0017] The mass ratio of the commercial molybdenum dioxide to the hydrogen peroxide solution is 1:(5-150); and / or

[0018] The oxidation reaction is first carried out by stirring at room temperature for 20 to 40 minutes, and then heated to 85°C to 95°C and stirred for 20 to 40 minutes; wherein, stirring at room temperature is to allow hydrogen peroxide and molybdenum disulfide to react fully, and heating and stirring are to remove excess hydrogen peroxide to avoid excessive pressure in the subsequent high-temperature and high-pressure hydrothermal reaction of hydrogen peroxide to avoid danger. In addition, heating may also further promote the oxidation reaction to be complete.

[0019] In the step of adding thiourea, a dispersant is also added; the dispersant is hexadecyl trimethyl ammonium bromide; the molar ratio of the commercial molybdenum dioxide to the hexadecyl trimethyl ammonium bromide is 1: (0.1-10); wherein the dispersant hexadecyl trimethyl ammonium bromide has excellent surface activity, stability and biodegradability, and has high compatibility with molybdenum disulfide. Moreover, since the dispersant is a cationic dispersant, and molybdenum disulfide has a layered structure of S-Mo-S and a negatively charged surface, hexadecyl trimethyl ammonium bromide can be dissolved in water and electrolyzed into organic ammonium ions and bromide ions in water, and the organic ammonium ions and the negatively charged molybdenum disulfide are coated with molybdenum disulfide through electrostatic adsorption, which avoids the agglomeration of layered molybdenum disulfide to a certain extent. And the dispersant is low in price and high in safety.

[0020] The molar ratio of the commercial molybdenum dioxide to the thiourea is 1:(1-3); and / or

[0021] The temperature of the hydrothermal reaction is 160° C. to 200° C., and the time of the hydrothermal reaction is 2 h to 4 h; and / or

[0022] The washing is performed by washing with water and ethanol alternately. The excess thiourea and dispersant can be washed away by washing with water and ethanol alternately. Since thiourea and dispersant hexadecyltrimethylammonium bromide are also organic substances and soluble in water and ethanol, washing with water and ethanol alternately is cleaner. Washing with ethanol is convenient for removing the water solvent and also convenient for subsequent drying.

[0023] In order to achieve the second purpose of the above invention, the technical solution adopted by the present invention is as follows:

[0024] The present invention provides an application of molybdenite to prepare micro-nano structured molybdenum disulfide. After the molybdenum ore is ground, the micro-nano structured molybdenum disulfide is prepared according to the above-mentioned preparation method of micro-nano structured molybdenum disulfide.

[0025] The application of molybdenite in the preparation of micro-nanostructured molybdenum disulfide can provide a method for the efficient utilization of molybdenite resources, which is a new way to efficiently utilize molybdenite resources. Through this application method, natural molybdenite resources can be more effectively utilized, and the application effect of photothermal hydrophobic materials in the field of anti-icing can be improved, providing new ideas and solutions for realizing green, environmentally friendly and efficient anti-icing technology.

[0026] In order to achieve the third purpose of the above invention, the technical solution adopted by the present invention is as follows:

[0027] The present invention provides a method for preparing a hydrophobic anti-icing coating based on molybdenum disulfide, wherein the micro-nanostructured molybdenum disulfide prepared by the above-mentioned method for preparing micro-nanostructured molybdenum disulfide comprises the following steps:

[0028] S1. Preparation of modified molybdenum disulfide: adding γ-aminopropyltriethoxysilane to a mixed solvent of water and ethanol for hydrolysis, then adding the micro-nanostructured molybdenum disulfide, stirring, washing, centrifuging and drying to obtain modified molybdenum disulfide;

[0029] S2. Preparation of a hydrophobic anti-icing coating: After dissolving polydimethylsiloxane in an organic solvent, add the modified molybdenum disulfide obtained in step S1, and mix well to obtain the hydrophobic anti-icing coating based on molybdenum disulfide.

[0030] The present invention discloses a method for preparing a hydrophobic anti-icing coating based on molybdenum disulfide, wherein the micro-nanostructured molybdenum disulfide prepared by the present invention is further modified by γ-aminopropyltriethoxysilane, that is, the micro-nanostructured molybdenum disulfide is grafted with a low surface energy compound polydimethylsiloxane by using the hydrolyzate of γ-aminopropyltriethoxysilane as a bridge, thereby obtaining a hydrophobic anti-icing coating with excellent photothermal conversion performance. Moreover, the hydrophobic anti-icing coating based on molybdenum disulfide prepared by the present invention can form an anti-icing coating with excellent photothermal function through the synergistic effect of modified molybdenum disulfide and fluorine-free polydimethylsiloxane, which is environmentally friendly, and its photothermal properties can effectively delay the anti-icing effect of the substrate. Moreover, the hydrophobic anti-icing coating based on molybdenum disulfide not only has a significant photothermal effect, can effectively prolong the freezing time of water, but also accelerate the melting process of frost. In addition, the use of fluorine-free material polydimethylsiloxane can avoid fluorine pollution to the environment, which is in line with the environmental protection concept of green chemistry.

[0031] Among them, the preparation mechanism of the hydrophobic anti-icing coating based on molybdenum disulfide is: there are a large number of hydroxyl groups on the surface of the micro-nanostructured molybdenum disulfide, which can react with the hydroxyl groups on the hydrolyzed γ-aminopropyltriethoxysilane, and then the amino groups on the γ-aminopropyltriethoxysilane are used to react with the hydroxyl groups on the polydimethylsiloxane to obtain the hydrophobic anti-icing coating based on molybdenum disulfide.

[0032] Among them, the preparation of modified molybdenum disulfide is carried out at room temperature and pressure, with the characteristics of mild conditions and simple process.

[0033] Furthermore, in step S1, the mass ratio of the γ-aminopropyltriethoxysilane, water, ethanol and micro-nanostructured molybdenum disulfide is (0.8-1.2):1:(15-20):(0.3-0.7); wherein, in the hydrolysis reaction, ethanol is used as a solvent for γ-aminopropyltriethoxysilane and water, which facilitates the dissolution of γ-aminopropyltriethoxysilane and also plays a good dispersing role, facilitating the hydrolysis reaction.

[0034] The hydrolysis time is 8 min to 12 min; and / or

[0035] The stirring is magnetic stirring, and the stirring time is 1.5h to 2.5h; and / or

[0036] The washing is performed using ethanol.

[0037] Furthermore, in step S2, the mass ratio of the modified molybdenum disulfide, polydimethylsiloxane and organic solvent is (15-35):(20-30):(800-1000); and / or

[0038] The mixing operation is to perform ultrasonic treatment for 20 min to 40 min.

[0039] In order to achieve the fourth object of the above invention, the technical solution adopted by the present invention is as follows:

[0040] The present invention provides a hydrophobic anti-icing coating based on molybdenum disulfide, which is prepared by the above-mentioned preparation method of the hydrophobic anti-icing coating based on molybdenum disulfide.

[0041] The present invention discloses a hydrophobic anti-icing coating based on molybdenum disulfide, which can form an anti-icing coating with excellent photothermal function through the synergistic effect of modified molybdenum disulfide and fluorine-free polydimethylsiloxane, is environmentally friendly, and its photothermal properties can effectively delay the anti-icing effect of the substrate. Moreover, the hydrophobic anti-icing coating based on molybdenum disulfide not only has a significant photothermal effect, can effectively prolong the freezing time of water, but also accelerate the melting process of frost. In addition, the use of fluorine-free material polydimethylsiloxane can avoid fluorine pollution to the environment, which is in line with the environmental protection concept of green chemistry.

[0042] In order to achieve the fifth purpose of the above invention, the technical solution adopted by the present invention is as follows:

[0043] The present invention provides an application of a hydrophobic anti-icing coating based on molybdenum disulfide. The hydrophobic anti-icing coating based on molybdenum disulfide prepared by the above-mentioned preparation method of the hydrophobic anti-icing coating based on molybdenum disulfide is sprayed on the surface of a substrate, and after drying and curing, the hydrophobic anti-icing coating based on molybdenum disulfide is obtained.

[0044] The invention discloses an application of a hydrophobic anti-icing coating based on molybdenum disulfide, which is sprayed on the surface of a substrate to prepare a hydrophobic anti-icing coating. The photothermal properties of the hydrophobic anti-icing coating can effectively delay the anti-icing effect of the substrate and accelerate the melting process of frost.

[0045] Furthermore, the spraying pressure is 3MPa to 5MPa; and / or

[0046] The drying and curing temperature is 75° C. to 85° C., and the drying and curing time is 1.5 h to 2.2 h.

[0047] Among them, the sprayed hydrophobic anti-icing coating based on molybdenum disulfide has different viscosities when cured at different temperatures due to the micro-nanostructured molybdenum disulfide grafted with γ-aminopropyltriethoxysilane and polydimethylsiloxane. In addition, considering that the hydrophobic anti-icing coating must have hydrophobic properties, the curing temperature is controlled at 75°C ~ 85°C, and the curing time is 1.5h ~ 2.2h, which is a better condition.

[0048] Furthermore, the substrate includes a metal substrate or a non-metal substrate; wherein the metal substrate is, for example, an aluminum sheet, stainless steel, etc.; the non-metal substrate is, for example, a paper-based material, etc.

[0049] When the substrate is a metal substrate, the surface of the metal substrate is pretreated and then sprayed with the molybdenum disulfide-based hydrophobic anti-icing coating;

[0050] The method for surface pretreatment of a metal substrate comprises the following steps: polishing the surface of the metal substrate with sandpaper, then ultrasonically washing it with ethanol and acetone in sequence, drying it, and then immersing the metal substrate in a mixed solution formed by mixing a dopamine hydrochloride solution and a Tris-HCl buffer solution to precipitate dopamine on the surface of the metal substrate, thereby completing the surface pretreatment of the metal substrate.

[0051] Among them, 500-grit sandpaper is used for grinding.

[0052] The concentration of the dopamine hydrochloride solution is 4 g / L, the concentration of the Tris-HCl buffer solution is 2.4 g / L, and the pH of the mixed solution is 4.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] (1) The preparation method of the micro-nanostructured molybdenum disulfide of the present invention is to pre-treat the commercial large-sized molybdenum disulfide particles with hydrogen peroxide, add thiourea as a new sulfur source, and convert the commercial molybdenum disulfide into molybdenum disulfide with a special morphology by a hydrothermal synthesis method, and the average size of the prepared molybdenum disulfide is about 300nm. Among them, the commercial molybdenum disulfide is added to a hydrogen peroxide solution for oxidation reaction, and the sulfur is removed in the form of hydrogen sulfide. At this time, there is only Mo source in the system, and thiourea is subsequently added as a sulfur source to re-synthesize molybdenum disulfide. That is, the preparation method can change the morphology of commercial molybdenum disulfide through simple processing steps, and the sulfur source is added again after the sulfur of molybdenum disulfide is removed by oxidation reaction, which can greatly reduce the size of molybdenum disulfide and reach nanometer size, so it can provide a good way for the subsequent utilization of molybdenite. Moreover, the entire process of the preparation method of the micro-nanostructured molybdenum disulfide is simple, the method is simple, the preparation cost is low, and the preparation efficiency is high. It realizes the nano-scaling of large-sized molybdenum disulfide and significantly improves the photothermal effect.

[0055] (2) The application of molybdenite in the preparation of micro-nanostructured molybdenum disulfide of the present invention can provide a method for the efficient utilization of molybdenite resources, which is a new way to efficiently utilize molybdenite resources. Through this application method, natural molybdenite resources can be more effectively utilized, and the application effect of photothermal hydrophobic materials in the field of anti-icing can be improved, providing new ideas and solutions for realizing green, environmentally friendly and efficient anti-icing technology. The low-energy consumption and high-efficiency production process of this application method conforms to the concept of low-carbon environmental protection and green life, has significant practical application value, and shows far-reaching social value and application potential.

[0056] (3) A method for preparing a hydrophobic anti-icing coating based on molybdenum disulfide of the present invention, wherein the micro-nanostructured molybdenum disulfide prepared by the present invention is further modified by using γ-aminopropyltriethoxysilane, that is, the micro-nanostructured molybdenum disulfide is grafted with a low surface energy compound polydimethylsiloxane through the hydrolyzate of γ-aminopropyltriethoxysilane as a bridge, thereby obtaining a hydrophobic anti-icing coating with excellent photothermal conversion performance. In addition, the hydrophobic anti-icing coating based on molybdenum disulfide prepared by the present invention can form an anti-icing coating with excellent photothermal function through the synergistic effect of modified molybdenum disulfide and fluorine-free polydimethylsiloxane, which is environmentally friendly, and its photothermal properties can effectively delay the anti-icing effect of the substrate. Moreover, the hydrophobic anti-icing coating based on molybdenum disulfide not only has a significant photothermal effect, can effectively prolong the freezing time of water, but also accelerate the melting process of frost. In addition, the use of fluorine-free material polydimethylsiloxane can avoid fluorine pollution to the environment, which is in line with the environmental protection concept of green chemistry.

[0057] (4) The present invention is a hydrophobic anti-icing coating based on molybdenum disulfide. Through the synergistic effect of modified molybdenum disulfide and fluorine-free polydimethylsiloxane, an anti-icing coating with excellent photothermal function can be formed, which is environmentally friendly, and its photothermal properties can effectively delay the anti-icing effect of the substrate. Moreover, the hydrophobic anti-icing coating based on molybdenum disulfide not only has a significant photothermal effect, can effectively prolong the freezing time of water, but also accelerate the melting process of frost. In addition, the use of fluorine-free material polydimethylsiloxane can avoid fluorine pollution to the environment, which is in line with the environmental protection concept of green chemistry.

[0058] (5) An application of a hydrophobic anti-icing coating based on molybdenum disulfide of the present invention is to spray the hydrophobic anti-icing coating based on molybdenum disulfide on the surface of a substrate, and to prepare a hydrophobic anti-icing coating. The photothermal properties of the hydrophobic anti-icing coating can effectively delay the anti-icing effect of the substrate, and can also accelerate the melting process of frost. In addition, the prepared hydrophobic anti-icing coating has hydrophobic properties, and its contact angle is 103°-130°. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0060] Figure 1 This is a SEM image of commercial molybdenum dioxide.

[0061] Figure 2 This is a SEM image of the micro-nanostructured molybdenum disulfide of Example 1 of the present invention.

[0062] Figure 3 This is a SEM image of the micro-nanostructured molybdenum disulfide of Example 2 of the present invention.

[0063] Figure 4 It is the XRD diagram of commercial molybdenum disulfide, the micro-nanostructured molybdenum disulfide prepared in Example 1, and the micro-nanostructured molybdenum disulfide prepared in Example 2.

[0064] Figure 5 It is an infrared spectra of the micro-nanostructured molybdenum disulfide prepared in Example 1, the modified molybdenum disulfide prepared in Example 8, and the hydrophobic anti-icing coating based on molybdenum disulfide prepared in Example 8.

[0065] Figure 6 This is a graph showing the contact angle test results of the hydrophobic anti-icing coating based on molybdenum disulfide prepared in Examples 11, 12, and 14-21.

[0066] Figure 7 This is a graph showing the test results of the delayed freezing time of the molybdenum disulfide-based hydrophobic anti-icing coating prepared in Examples 11, 12, and 14-21.

[0067] Figure 8 This is a graph showing the surface photothermal effect performance test results of a blank aluminum sheet, an aluminum sheet treated with polydimethylsiloxane, and a hydrophobic anti-icing coating based on molybdenum disulfide prepared in Example 11. DETAILED DESCRIPTION

[0068] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0069] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. In the present invention, the singular forms "a", "said" and "the" used in the embodiments and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0070] In an embodiment of the present invention, a method for preparing micro-nanostructured molybdenum disulfide comprises the following steps: adding commercial molybdenum dioxide to a hydrogen peroxide solution for oxidation reaction, then adding thiourea, placing the mixture in a hydrothermal reactor for hydrothermal reaction, and then washing and drying to obtain the micro-nanostructured molybdenum disulfide.

[0071] The preparation method of the micro-nano structured molybdenum disulfide of the present invention is to use hydrogen peroxide to perform oxidation pretreatment on commercial large-sized molybdenum disulfide particles, add thiourea as a new sulfur source, and convert the commercial molybdenum disulfide into molybdenum disulfide with a special morphology through a hydrothermal synthesis method, and the average size of the prepared molybdenum disulfide is about 300nm. Among them, the commercial molybdenum disulfide is added to a hydrogen peroxide solution for oxidation reaction, and the sulfur is removed in the form of hydrogen sulfide. At this time, there is only a Mo source in the system, and thiourea is subsequently added as a sulfur source to resynthesize molybdenum disulfide, that is, the preparation method can change the morphology of commercial molybdenum disulfide through simple processing steps, and after the sulfur of molybdenum disulfide is removed by oxidation reaction first and then the sulfur source is re-added, the size of molybdenum disulfide can be greatly reduced and reach the nanometer size, so it can provide a good way for the subsequent use of molybdenite. In addition, the whole process of the preparation method of the micro-nano structured molybdenum disulfide is simple, the preparation cost is low, and the preparation efficiency is high, and the nanometerization of large-sized molybdenum disulfide is realized.

[0072] Among them, using hydrogen peroxide as an oxidant also has the advantages of low cost and being green and environmentally friendly.

[0073] In the embodiment of the present invention, the size of the commercial molybdenum dioxide is 5 μm to 30 μm; and / or

[0074] In some embodiments, the mass concentration of the hydrogen peroxide solution is 8% to 12%; and / or

[0075] The mass ratio of the commercial molybdenum dioxide to the hydrogen peroxide solution is 1:(5-150); and / or

[0076] In some embodiments, the oxidation reaction is first carried out by stirring at room temperature for 20 to 40 minutes, and then heated to 85°C to 95°C and stirred for 20 to 40 minutes; wherein, stirring at room temperature is to allow hydrogen peroxide and molybdenum disulfide to react fully, and heating and stirring are to remove excess hydrogen peroxide to avoid excessive pressure in the subsequent high-temperature and high-pressure hydrothermal reaction of hydrogen peroxide to avoid danger. In addition, heating may also further promote the oxidation reaction to be complete.

[0077] In some embodiments, a dispersant is also added in the step of adding thiourea; the dispersant is hexadecyl trimethyl ammonium bromide; the molar ratio of the commercial molybdenum dioxide to the hexadecyl trimethyl ammonium bromide is 1: (0.1-10); wherein the dispersant hexadecyl trimethyl ammonium bromide has excellent surface activity, stability and biodegradability, and has high compatibility with molybdenum disulfide. Moreover, since the dispersant is a cationic dispersant, and molybdenum disulfide has a layered structure of S-Mo-S and a negatively charged surface, hexadecyl trimethyl ammonium bromide can be dissolved in water and electrolyzed into organic ammonium ions and bromide ions in water, and the organic ammonium ions and negatively charged molybdenum disulfide are coated with molybdenum disulfide through electrostatic adsorption, which avoids the agglomeration of layered molybdenum disulfide to a certain extent. And the dispersant is low in price and high in safety.

[0078] In some embodiments, the molar ratio of the commercial molybdenum dioxide to the thiourea is 1:(1-3); and / or

[0079] In some embodiments, the temperature of the hydrothermal reaction is 160° C. to 200° C., and the time of the hydrothermal reaction is 2 h to 4 h; and / or

[0080] The washing is performed by washing with water and ethanol alternately. The excess thiourea and dispersant can be washed away by washing with water and ethanol alternately. Since thiourea and dispersant hexadecyltrimethylammonium bromide are also organic substances and soluble in water and ethanol, washing with water and ethanol alternately is cleaner. Washing with ethanol is convenient for removing the water solvent and also convenient for subsequent drying.

[0081] In the embodiment of the present invention, molybdenite is used to prepare micro-nanostructured molybdenum disulfide. After the molybdenite is ground, the micro-nanostructured molybdenum disulfide is prepared according to the above-mentioned preparation method of micro-nanostructured molybdenum disulfide.

[0082] The application of molybdenite in the embodiment to prepare micro-nanostructured molybdenum disulfide can provide a method for the efficient utilization of molybdenite resources, which is a new way to efficiently utilize molybdenite resources. Through this application method, natural molybdenite resources can be more effectively utilized, the application effect of photothermal hydrophobic materials in the field of anti-icing can be improved, and new ideas and solutions can be provided for realizing green, environmentally friendly and efficient anti-icing technology.

[0083] In an embodiment of the present invention, a method for preparing a hydrophobic anti-icing coating based on molybdenum disulfide, wherein the micro-nanostructured molybdenum disulfide prepared by the above-mentioned method for preparing micro-nanostructured molybdenum disulfide, comprises the following steps:

[0084] S1. Preparation of modified molybdenum disulfide: adding γ-aminopropyltriethoxysilane to a mixed solvent of water and ethanol for hydrolysis, then adding the micro-nanostructured molybdenum disulfide, stirring, washing, centrifuging and drying to obtain modified molybdenum disulfide;

[0085] S2. Preparation of a hydrophobic anti-icing coating: After dissolving polydimethylsiloxane in an organic solvent, add the modified molybdenum disulfide obtained in step S1, and mix well to obtain the hydrophobic anti-icing coating based on molybdenum disulfide.

[0086] A preparation method of a hydrophobic anti-icing coating based on molybdenum disulfide in the embodiment, by further modifying the micro-nanostructured molybdenum disulfide prepared by the present invention using γ-aminopropyltriethoxysilane, that is, the micro-nanostructured molybdenum disulfide is grafted with a low surface energy compound polydimethylsiloxane through the hydrolyzate of γ-aminopropyltriethoxysilane as a bridge, thereby obtaining a hydrophobic anti-icing coating with excellent photothermal conversion performance. In addition, the hydrophobic anti-icing coating based on molybdenum disulfide prepared by the present invention can form an anti-icing coating with excellent photothermal function through the synergistic effect of modified molybdenum disulfide and fluorine-free polydimethylsiloxane, which is environmentally friendly, and its photothermal properties can effectively delay the anti-icing effect of the substrate. Moreover, the hydrophobic anti-icing coating based on molybdenum disulfide not only has a significant photothermal effect, can effectively prolong the freezing time of water, but also accelerate the melting process of frost. In addition, the use of fluorine-free material polydimethylsiloxane can avoid fluorine pollution to the environment, which is in line with the environmental protection concept of green chemistry.

[0087] Among them, the preparation mechanism of the hydrophobic anti-icing coating based on molybdenum disulfide is: there are a large number of hydroxyl groups on the surface of the micro-nanostructured molybdenum disulfide, which can react with the hydroxyl groups on the hydrolyzed γ-aminopropyltriethoxysilane, and then the amino groups on the γ-aminopropyltriethoxysilane are used to react with the hydroxyl groups on the polydimethylsiloxane to obtain the hydrophobic anti-icing coating based on molybdenum disulfide.

[0088] Among them, the preparation of modified molybdenum disulfide is carried out at room temperature and pressure, with the characteristics of mild conditions and simple process.

[0089] In some embodiments, in step S1, the mass ratio of γ-aminopropyltriethoxysilane, water, ethanol and micro-nanostructured molybdenum disulfide is (0.8-1.2):1:(15-20):(0.3-0.7); wherein, in the hydrolysis reaction, ethanol serves as a solvent for γ-aminopropyltriethoxysilane and water, which facilitates the dissolution of γ-aminopropyltriethoxysilane and also plays a good dispersing role, facilitating the hydrolysis reaction.

[0090] In some embodiments, the hydrolysis time is 8 min to 12 min; and / or

[0091] The stirring is magnetic stirring, and the stirring time is 1.5h to 2.5h; and / or

[0092] The washing is performed using ethanol.

[0093] In some embodiments, in step S2, the mass ratio of the modified molybdenum disulfide, polydimethylsiloxane and organic solvent is (15-35):(20-30):(800-1000); and / or

[0094] The mixing operation is to perform ultrasonic treatment for 20 min to 40 min.

[0095] In an embodiment of the present invention, a hydrophobic anti-icing coating based on molybdenum disulfide is prepared by the above-mentioned preparation method of a hydrophobic anti-icing coating based on molybdenum disulfide.

[0096] A hydrophobic anti-icing coating based on molybdenum disulfide in the embodiment can form an anti-icing coating with excellent photothermal function through the synergistic effect of modified molybdenum disulfide and fluorine-free polydimethylsiloxane, which is environmentally friendly, and its photothermal properties can effectively delay the anti-icing effect of the substrate. Moreover, the hydrophobic anti-icing coating based on molybdenum disulfide not only has a significant photothermal effect, can effectively prolong the freezing time of water, but also accelerate the melting process of frost. In addition, the use of fluorine-free material polydimethylsiloxane can avoid fluorine pollution to the environment, which is in line with the environmental protection concept of green chemistry.

[0097] In an embodiment of the present invention, an application of a hydrophobic anti-icing coating based on molybdenum disulfide is provided. The hydrophobic anti-icing coating based on molybdenum disulfide obtained by the preparation method of the hydrophobic anti-icing coating based on molybdenum disulfide described above is sprayed on the surface of a substrate, and after drying and curing, a hydrophobic anti-icing coating based on molybdenum disulfide is obtained.

[0098] In one embodiment, the application of the hydrophobic anti-icing coating based on molybdenum disulfide is to spray the hydrophobic anti-icing coating based on molybdenum disulfide on the surface of the substrate to prepare the hydrophobic anti-icing coating. The photothermal properties of the hydrophobic anti-icing coating can effectively delay the anti-icing effect of the substrate and accelerate the melting process of frost.

[0099] In some embodiments, the spraying pressure is 3MPa to 5MPa; and / or

[0100] The drying and curing temperature is 75° C. to 85° C., and the drying and curing time is 1.5 h to 2.2 h.

[0101] Among them, the sprayed hydrophobic anti-icing coating based on molybdenum disulfide has different viscosities when cured at different temperatures due to the micro-nanostructured molybdenum disulfide grafted with γ-aminopropyltriethoxysilane and polydimethylsiloxane. In addition, considering that the hydrophobic anti-icing coating must have hydrophobic properties, the curing temperature is controlled at 75°C ~ 85°C, and the curing time is 1.5h ~ 2.2h, which is a better condition.

[0102] In some embodiments, the substrate includes a metal substrate or a non-metal substrate; wherein the metal substrate is, for example, an aluminum sheet, stainless steel, etc.; the non-metal substrate is, for example, a paper-based material, etc.

[0103] When the substrate is a metal substrate, the surface of the metal substrate is pretreated and then sprayed with the molybdenum disulfide-based hydrophobic anti-icing coating;

[0104] The method for surface pretreatment of a metal substrate comprises the following steps: polishing the surface of the metal substrate with sandpaper, then ultrasonically washing it with ethanol and acetone in sequence, drying it, and then immersing the metal substrate in a mixed solution formed by mixing a dopamine hydrochloride solution and a Tris-HCl buffer solution to precipitate dopamine on the surface of the metal substrate, thereby completing the surface pretreatment of the metal substrate.

[0105] In some embodiments, 500 grit sandpaper is used for sanding.

[0106] In some embodiments, the concentration of the dopamine hydrochloride solution is 4 g / L, the concentration of the Tris-HCl buffer solution is 2.4 g / L, and the pH of the mixed solution is 4.

[0107] The following describes the invention in conjunction with specific embodiments.

[0108] Example 1

[0109] The preparation method of micro-nano structured molybdenum disulfide comprises the following steps: adding commercial molybdenum dioxide to a hydrogen peroxide solution with a mass concentration of 10% to carry out an oxidation reaction, first stirring at room temperature for 30 minutes, then heating to 90° C. and stirring for 30 minutes; then adding thiourea, placing in a polytetrafluoroethylene hydrothermal reactor at 180° C. for hydrothermal reaction for 2 hours, then washing with water and ethanol alternately, and drying to obtain the micro-nano structured molybdenum disulfide.

[0110] Among them, the size of commercial molybdenum dioxide is 5μm to 30μm.

[0111] In this embodiment, the mass ratio of commercial molybdenum dioxide to hydrogen peroxide solution is 1:10; the molar ratio of commercial molybdenum dioxide to thiourea is 1:2.

[0112] Example 2

[0113] The preparation method of micro-nano structured molybdenum disulfide comprises the following steps: adding commercial molybdenum dioxide to a hydrogen peroxide solution with a mass concentration of 10% to carry out an oxidation reaction, first stirring at room temperature for 30 minutes, then heating to 90° C. and stirring for 30 minutes; then adding thiourea and a dispersant, placing in a hydrothermal reactor at 180° C. for a hydrothermal reaction for 2 hours, then washing with water and ethanol alternately, and drying to obtain the micro-nano structured molybdenum disulfide.

[0114] Among them, the size of commercial molybdenum dioxide is 5μm to 30μm.

[0115] In this embodiment, the mass ratio of commercial molybdenum dioxide to hydrogen peroxide solution is 1:10; the molar ratio of commercial molybdenum dioxide to thiourea is 1:2.

[0116] In this embodiment, the dispersant is hexadecyltrimethylammonium bromide; the molar ratio of commercial molybdenum dioxide to hexadecyltrimethylammonium bromide is 1:1.

[0117] Example 3

[0118] The preparation method of micro-nano structured molybdenum disulfide comprises the following steps: adding commercial molybdenum dioxide to a hydrogen peroxide solution with a mass concentration of 8% to carry out an oxidation reaction, first stirring at room temperature for 20 minutes, then heating to 85°C and stirring for 40 minutes; then adding thiourea and a dispersant, placing in a hydrothermal reactor at 160°C for a hydrothermal reaction for 4 hours, then washing with water and ethanol alternately, and drying to obtain the micro-nano structured molybdenum disulfide.

[0119] Among them, the size of commercial molybdenum dioxide is 5μm to 30μm.

[0120] In this embodiment, the mass ratio of commercial molybdenum dioxide to hydrogen peroxide solution is 1:5; the molar ratio of commercial molybdenum dioxide to thiourea is 1:1.

[0121] In this embodiment, the dispersant is hexadecyltrimethylammonium bromide; the molar ratio of commercial molybdenum dioxide to hexadecyltrimethylammonium bromide is 1:0.1.

[0122] Example 4

[0123] The preparation method of micro-nano structured molybdenum disulfide comprises the following steps: adding commercial molybdenum dioxide to a hydrogen peroxide solution with a mass concentration of 12% for oxidation reaction, first stirring at room temperature for 40 minutes, then heating to 95°C and stirring for 20 minutes; then adding thiourea and a dispersant, placing in a hydrothermal reactor for hydrothermal reaction at 200°C for 3 hours, then washing with water and ethanol alternately, and drying to obtain the micro-nano structured molybdenum disulfide.

[0124] Among them, the size of commercial molybdenum dioxide is 5μm to 30μm.

[0125] In this embodiment, the mass ratio of commercial molybdenum dioxide to hydrogen peroxide solution is 1:150; the molar ratio of commercial molybdenum dioxide to thiourea is 1:3.

[0126] In this embodiment, the dispersant is hexadecyltrimethylammonium bromide; the molar ratio of commercial molybdenum dioxide to hexadecyltrimethylammonium bromide is 1:10.

[0127] Example 5

[0128] Preparation method of micro-nanostructured molybdenum disulfide. The difference between this embodiment and Example 2 is that the molar ratio of commercial molybdenum dioxide to hexadecyltrimethylammonium bromide in this embodiment is 1:3, and the remaining components and preparation method are the same as those in Example 2.

[0129] Example 6

[0130] Preparation method of micro-nanostructured molybdenum disulfide. The difference between this embodiment and Example 2 is that the molar ratio of commercial molybdenum dioxide to hexadecyltrimethylammonium bromide in this embodiment is 1:6, and the remaining components and preparation method are the same as those in Example 2.

[0131] Example 7

[0132] The application of molybdenite in preparing micro-nanostructured molybdenum disulfide is to grind the molybdenite and then prepare the micro-nanostructured molybdenum disulfide according to the preparation method of micro-nanostructured molybdenum disulfide in any one of Examples 1 to 6.

[0133] Example 8

[0134] A method for preparing a hydrophobic anti-icing coating based on molybdenum disulfide, using the micro-nanostructured molybdenum disulfide prepared in Example 1, comprising the following steps:

[0135] S1. Preparation of modified molybdenum disulfide: After adding γ-aminopropyltriethoxysilane to a mixed solvent of water and ethanol for hydrolysis for 10 minutes, the micro-nanostructured molybdenum disulfide is added, followed by magnetic stirring for 2 hours, washing with ethanol, centrifugation and drying to obtain modified molybdenum disulfide; in this embodiment, the mass ratio of γ-aminopropyltriethoxysilane, water, ethanol and micro-nanostructured molybdenum disulfide is 1:1:18:0.5;

[0136] S2, preparation of hydrophobic anti-icing coating: After dissolving polydimethylsiloxane in an organic solvent, adding the modified molybdenum disulfide prepared in step S1, ultrasonically treating and mixing for 30 minutes, the hydrophobic anti-icing coating based on molybdenum disulfide is prepared. In this embodiment, the mass ratio of modified molybdenum disulfide, polydimethylsiloxane and organic solvent is 30:25:900.

[0137] Example 9

[0138] A method for preparing a hydrophobic anti-icing coating based on molybdenum disulfide, using the micro-nanostructured molybdenum disulfide prepared in Example 2, comprises the following steps:

[0139] S1. Preparation of modified molybdenum disulfide: γ-aminopropyltriethoxysilane was added to a mixed solvent of water and ethanol for hydrolysis for 8 minutes, and then the micro-nanostructured molybdenum disulfide was added, followed by magnetic stirring for 1.5 hours, washing with ethanol, centrifugation and drying to obtain modified molybdenum disulfide; in this embodiment, the mass ratio of γ-aminopropyltriethoxysilane, water, ethanol and micro-nanostructured molybdenum disulfide was 0.8:1:15:0.3;

[0140] S2, preparation of hydrophobic anti-icing coating: After dissolving polydimethylsiloxane in an organic solvent, adding the modified molybdenum disulfide prepared in step S1, ultrasonically treating and mixing for 20 minutes, the hydrophobic anti-icing coating based on molybdenum disulfide is prepared. In this embodiment, the mass ratio of modified molybdenum disulfide, polydimethylsiloxane and organic solvent is 15:20:800.

[0141] Example 10

[0142] A method for preparing a hydrophobic anti-icing coating based on molybdenum disulfide, using the micro-nanostructured molybdenum disulfide prepared in Example 3, comprises the following steps:

[0143] S1. Preparation of modified molybdenum disulfide: After adding γ-aminopropyltriethoxysilane to a mixed solvent of water and ethanol for hydrolysis for 12 minutes, the micro-nanostructured molybdenum disulfide is added, followed by magnetic stirring for 2.5 hours, washing with ethanol, centrifugation and drying to obtain modified molybdenum disulfide; in this embodiment, the mass ratio of γ-aminopropyltriethoxysilane, water, ethanol and micro-nanostructured molybdenum disulfide is 1.2:1:20:0.7;

[0144] S2, preparation of hydrophobic anti-icing coating: After dissolving polydimethylsiloxane in an organic solvent, adding the modified molybdenum disulfide prepared in step S1, ultrasonically treating and mixing for 40 minutes, the hydrophobic anti-icing coating based on molybdenum disulfide is prepared. In this embodiment, the mass ratio of modified molybdenum disulfide, polydimethylsiloxane and organic solvent is 35:30:1000.

[0145] Embodiment 11

[0146] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The hydrophobic anti-icing coating based on molybdenum disulfide prepared by the preparation method of a hydrophobic anti-icing coating based on molybdenum disulfide in Example 8 is sprayed on the surface of an aluminum sheet, and then dried and cured at 80°C for 2 hours to obtain a hydrophobic anti-icing coating based on molybdenum disulfide.

[0147] In this embodiment, the spraying pressure is 3 MPa; the spraying cycle is 1 time, that is, one layer of coating; wherein, in each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 .

[0148] Before spraying, the surface of the aluminum sheet was polished with 500-mesh sandpaper, and then ultrasonically cleaned with ethanol and acetone in sequence, dried, and then immersed in a mixed solution of pH=4 formed by mixing a 4 g / L dopamine hydrochloride solution with a concentration of 2.4 g / L Tris-HCl buffer solution to precipitate dopamine on the surface of the aluminum sheet, thereby completing the surface pretreatment of the aluminum sheet.

[0149] Example 12

[0150] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The hydrophobic anti-icing coating based on molybdenum disulfide prepared by the preparation method of a hydrophobic anti-icing coating based on molybdenum disulfide in Example 9 is sprayed on the surface of an aluminum sheet, and then dried and cured at 75°C for 2.2 hours to obtain a hydrophobic anti-icing coating based on molybdenum disulfide.

[0151] In this embodiment, the spraying pressure is 4 MPa; the spraying cycle is 1 time, that is, one layer of coating; wherein, in each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 .

[0152] Before spraying, the surface of the aluminum sheet was polished with 500-mesh sandpaper, and then ultrasonically cleaned with ethanol and acetone in sequence, dried, and then immersed in a mixed solution of pH=4 formed by mixing a 4 g / L dopamine hydrochloride solution with a concentration of 2.4 g / L Tris-HCl buffer solution to precipitate dopamine on the surface of the aluminum sheet, thereby completing the surface pretreatment of the aluminum sheet.

[0153] Embodiment 13

[0154] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The hydrophobic anti-icing coating based on molybdenum disulfide prepared by the preparation method of a hydrophobic anti-icing coating based on molybdenum disulfide in Example 10 is sprayed on the surface of an aluminum sheet, and then dried and cured at 85°C for 1.5 hours to obtain a hydrophobic anti-icing coating based on molybdenum disulfide.

[0155] In this embodiment, the spraying pressure is 5 MPa; the spraying cycle is 1 time, that is, a layer of coating; wherein, in each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 .

[0156] Before spraying, the surface of the aluminum sheet was polished with 500-mesh sandpaper, and then ultrasonically cleaned with ethanol and acetone in sequence, dried, and then immersed in a mixed solution of pH=4 formed by mixing a 4 g / L dopamine hydrochloride solution with a concentration of 2.4 g / L Tris-HCl buffer solution to precipitate dopamine on the surface of the aluminum sheet, thereby completing the surface pretreatment of the aluminum sheet.

[0157] Embodiment 14

[0158] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The difference between this embodiment and embodiment 11 is that the spraying cycle is 2 times, that is, 2 layers of coating. In each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 The remaining conditions, parameters and methods of this embodiment are the same as those of embodiment 11.

[0159] Embodiment 15

[0160] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The difference between this embodiment and embodiment 11 is that the spraying cycle is 3 times, that is, 3 layers of coating. In each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 The remaining conditions, parameters and methods of this embodiment are the same as those of embodiment 11.

[0161] Example 16

[0162] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The difference between this embodiment and embodiment 11 is that the spraying cycle is 4 times, that is, 4 layers of coating. In each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 The remaining conditions, parameters and methods of this embodiment are the same as those of embodiment 11.

[0163] Embodiment 17

[0164] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The difference between this embodiment and embodiment 11 is that the spraying cycle is 5 times, that is, 5 layers of coating. In each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 The remaining conditions, parameters and methods of this embodiment are the same as those of embodiment 11.

[0165] Embodiment 18

[0166] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The difference between this embodiment and embodiment 12 is that the spraying cycle is 2 times, that is, 2 layers of coating. In each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 The remaining conditions, parameters and methods of this embodiment are the same as those of embodiment 12.

[0167] Embodiment 19

[0168] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The difference between this embodiment and embodiment 12 is that the spraying cycle is 3 times, that is, 3 layers of coating. In each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 The remaining conditions, parameters and methods of this embodiment are the same as those of embodiment 12.

[0169] Embodiment 20

[0170] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The difference between this embodiment and embodiment 12 is that the spraying cycle is 4 times, that is, 4 layers of coating. In each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 The remaining conditions, parameters and methods of this embodiment are the same as those of embodiment 12.

[0171] Embodiment 21

[0172] An application of a hydrophobic anti-icing coating based on molybdenum disulfide. The difference between this embodiment and embodiment 12 is that the spraying cycle is 5 times, that is, 5 layers of coating. In each layer of coating, the amount of the hydrophobic anti-icing coating based on molybdenum disulfide is 6.25 mg / cm 2 The remaining conditions, parameters and methods of this embodiment are the same as those of embodiment 12.

[0173] Structural morphology characterization

[0174] (I) Morphological characterization by scanning electron microscopy

[0175] The micro-nanostructured molybdenum disulfide prepared by the preparation method of micro-nanostructured molybdenum disulfide in Example 1 was characterized by scanning electron microscopy (SEM). Figure 2 shown.

[0176] from Figure 2 It can be seen that the micro-nanostructured molybdenum disulfide prepared by the preparation method of the micro-nanostructured molybdenum disulfide of the present invention is superior to commercial molybdenum disulfide (such as Figure 1As shown in the figure, the particle size is reduced from micrometer level to nanometer level, the size is greatly reduced, the average size is about 300nm, the specific surface area is greatly increased, and the photothermal effect can be significantly improved. It can be seen that the preparation method of the micro-nanostructured molybdenum disulfide of this embodiment changes the morphology of commercial molybdenum disulfide. The particle size of the molybdenum disulfide synthesized by the hydrothermal method is significantly reduced, the dispersibility is better, and fine rough micro-nano protrusions are formed on the surface.

[0177] The micro-nanostructured molybdenum disulfide prepared by the preparation method of micro-nanostructured molybdenum disulfide in Example 2 was characterized by scanning electron microscopy (SEM). Figure 3 shown.

[0178] from Figure 3 It can be seen that the preparation method of the micro-nanostructured molybdenum disulfide of the present invention, while adding thiourea, adds the dispersant hexadecyltrimethylammonium bromide (CTAB), which can make the crystal surface of the prepared micro-nanostructured molybdenum disulfide smoother and controlled within the range of nanometer size. The particles thereof are also relatively free of rough protrusions on the surface, the surface is smoother, the particles are larger, and the crystal structure is more regular, which can better enhance the photothermal effect and better delay the freezing time.

[0179] (II) XRD structural characterization

[0180] The commercial molybdenum disulfide, the micro-nanostructured molybdenum disulfide prepared in Example 1, and the micro-nanostructured molybdenum disulfide prepared in Example 2 were characterized by XRD. Figure 4 shown.

[0181] Figure 4 In the figure, commercial MoS2 refers to commercial molybdenum disulfide, MoS2 refers to the micro-nanostructured molybdenum disulfide prepared in Example 1, and MoS2-CTAB refers to the micro-nanostructured molybdenum disulfide prepared in Example 2.

[0182] Depend on Figure 4 It can be seen that the XRD peak of commercial molybdenum disulfide corresponds to the XRD standard card number PDF#77-1716, proving that the commercial purchase is indeed molybdenum disulfide powder. The XRD peaks of the micro-nanostructured molybdenum disulfide synthesized by hydrothermal synthesis in Example 1 and the micro-nanostructured molybdenum disulfide synthesized by hydrothermal synthesis with the addition of a dispersant in Example 2 correspond to the XRD peaks of commercial molybdenum disulfide, indicating that molybdenum disulfide is successfully prepared by the method of adding thiourea for hydrothermal reaction after hydrogen peroxide oxidation. After the hydrothermal reaction, it can be clearly seen that the peak intensity has weakened, indicating that the crystallinity of the molybdenum disulfide after the hydrothermal reaction has weakened, the dispersibility has improved, and it is more conducive to exposing defects, making the surface hydrophobic, which is consistent with the characterization of SEM.

[0183] (III) Structural characterization by infrared spectroscopy

[0184] The micro-nanostructured molybdenum disulfide prepared in Example 1, the modified molybdenum disulfide prepared in Example 8, and the hydrophobic anti-icing coating based on molybdenum disulfide prepared in Example 8 were characterized by infrared spectroscopy. Figure 5 shown.

[0185] Figure 5 In the figure, MoS2 refers to the micro-nanostructured molybdenum disulfide prepared in Example 1, MoS2-APTES refers to the modified molybdenum disulfide prepared in Example 8, and MoS2-APTES-PDMS refers to the hydrophobic anti-icing coating based on molybdenum disulfide prepared in Example 8.

[0186] Figure 5 In the figure, the infrared absorption spectrum data of the above samples were tested using a full-band research-level infrared spectroscopy workstation produced by THEMOR-FILSHER in the United States, and the infrared absorption peaks of the micro-nanostructured molybdenum disulfide synthesized by hydrothermal synthesis in Example 1, the modified molybdenum disulfide prepared in Example 8, and the hydrophobic anti-icing coating based on molybdenum disulfide prepared in Example 8 were compared. In the figure, the large broad peak in the front is the hydroxyl group adsorbed on the surface of MoS2, with a wavelength of 1606.6 cm -1 It is the bending vibration peak of -OH adsorbed on the surface; wavelength 1500.3cm -1 The absorption peak of NH on the amino peak is at 1399.8 cm. The coupling agent γ-aminopropyltriethoxysilane has NH3 functional group. -1 It is a common peak of MoS2; wavelength 1029.5cm -1 The peak of Si-O-Si is at 565.6 cm -1 It is the Mo-S vibration peak of MoS2, which is all the peaks of MoS2. After the final modification, the hydrophobic anti-icing coating powder based on molybdenum disulfide can be seen to have NH and Si-O-Si, which can also indirectly prove the successful modification.

[0187] Performance Testing

[0188] (I) Hydrophobic performance test

[0189] The hydrophobic anti-icing coatings based on molybdenum disulfide prepared in Examples 11, 12, 14-21 were tested for contact angles. The video optical contact angle measuring instrument OCA100 produced by Dataphysics in Germany was used to test the wettability of the hydrophobic anti-icing coatings based on molybdenum disulfide prepared above. Five different positions were selected on the surface of each sample for measurement, and five measurement values ​​were obtained, and then the average of the five measurement values ​​was taken. The above contact angle test results are shown in Figure 1. Figure 6 shown.

[0190] from Figure 6It can be seen that the contact angles of the two samples sprayed with different numbers of layers (coating samples with dispersant added and coating samples without dispersant added) can reach about 110°, proving that the hydrophobicity and wettability of the above sample coatings are not much different.

[0191] (II) Anti-icing performance test

[0192] The hydrophobic anti-icing coatings based on molybdenum disulfide prepared in Examples 11, 12, and 14-21 were tested for their anti-icing performance. The delayed freezing time of the coatings of the above-mentioned embodiments was measured to determine the anti-icing performance of the coatings. The longer the delayed freezing time, the better the anti-icing performance. Among them, the delayed freezing time is the time it takes for a water droplet to transform from a liquid phase to a solid phase. It is recorded by a high-speed camera, the freezing temperature is set to -14°C, the humidity is maintained at 60%-80%, and 10uL of deionized water is taken with a pipette and dripped onto the surface of the coatings of different embodiments to measure the delayed freezing time, such as Figure 7 shown.

[0193] from Figure 7 It can be seen that, although the wettability of coatings with different numbers of spray layers is not much different in macroscopic terms, in the delayed freezing time test, it can be seen that with the increase in the number of layers, the delayed freezing time performance has a trend of first increasing and then decreasing, so that a more reasonable and reliable number of spray layers can be determined, that is, the spraying amount can be determined, and the experimental parameters can be further optimized. The experimental results show that the hydrothermally synthesized molybdenum disulfide coating with the addition of a dispersant has the best performance in the three-layer spraying.

[0194] (II) Surface photothermal effect performance test

[0195] The surface photothermal effect performance of a blank aluminum sheet, an aluminum sheet treated with polydimethylsiloxane, and a hydrophobic anti-icing coating based on molybdenum disulfide prepared in Example 11 were tested respectively. The aluminum sheet treated with polydimethylsiloxane refers to an aluminum sheet obtained by spraying polydimethylsiloxane on the surface of the aluminum sheet and curing it.

[0196] The surface photothermal effect performance test is to test the temperature change of the frost melting process on the surface of the test sample under the irradiation of the xenon lamp. The specific test process of the above three samples is: first freeze the three samples for more than 1 hour to form a frost layer of a certain thickness, set the freezing platform temperature at -20℃~-22℃, then turn on the xenon lamp, the current of the xenon lamp is set to 11A, and the light intensity is 500W / cm 2 , the test results are as follows Figure 8 shown.

[0197] Figure 8 In the figure, the PDMS curve represents the aluminum sheet treated with polydimethylsiloxane, and the MoS2 curve represents the hydrophobic anti-icing coating based on molybdenum disulfide prepared in Example 11.

[0198] Depend on Figure 8 It can be seen that, by comparison, under light irradiation, the hydrophobic anti-icing coating based on molybdenum disulfide prepared in the present invention can be heated to 0°C in 2 minutes, and reach a maximum temperature of 10°C in about 5 minutes, and can quickly melt ice. However, the temperature of the blank aluminum sheet and the aluminum sheet treated with polydimethylsiloxane reaches a temperature equilibrium after rising to -5°C, that is, it cannot rise any further, so it cannot melt ice.

[0199] Therefore, the hydrophobic anti-icing coating based on molybdenum disulfide prepared in the present invention has a significant photothermal effect and can melt ice quickly.

[0200] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing micro-nanostructured molybdenum disulfide, characterized in that: The following steps are involved: Commercial molybdenum dioxide is added to a hydrogen peroxide solution for oxidation reaction, and then thiourea is added, and the mixture is placed in a hydrothermal reactor for hydrothermal reaction, and then washed and dried to obtain the micro-nanostructured molybdenum disulfide.

2. The method for preparing micro-nanostructured molybdenum disulfide according to claim 1, characterized in that: The commercial molybdenum dioxide has a size of 5 μm to 30 μm; and / or The mass concentration of the hydrogen peroxide solution is 8% to 12%; and / or The mass ratio of the commercial molybdenum dioxide to the hydrogen peroxide solution is 1:(5-150); and / or The oxidation reaction is first carried out by stirring at room temperature for 20 to 40 minutes, and then heated to 85 to 95° C. and stirred for 20 to 40 minutes; and / or In the step of adding thiourea, a dispersant is also added; the dispersant is hexadecyltrimethylammonium bromide; the molar ratio of the commercial molybdenum dioxide to the hexadecyltrimethylammonium bromide is 1:(0.1-10); and / or The molar ratio of the commercial molybdenum dioxide to the thiourea is 1:(1-3); and / or The temperature of the hydrothermal reaction is 160° C. to 200° C., and the time of the hydrothermal reaction is 2 h to 4 h; and / or The washing is performed by alternating washing with water and ethanol.

3. The application of molybdenite in preparing micro-nanostructured molybdenum disulfide, characterized in that: After the molybdenite is ground, micro-nanostructured molybdenum disulfide is prepared according to the preparation method of micro-nanostructured molybdenum disulfide according to any one of claims 1 to 2.

4. A method for preparing a hydrophobic anti-icing coating based on molybdenum disulfide, characterized in that: The micro-nanostructured molybdenum disulfide prepared by the preparation method of the micro-nanostructured molybdenum disulfide according to any one of claims 1 to 2 comprises the following steps: S1. Preparation of modified molybdenum disulfide: adding γ-aminopropyltriethoxysilane to a mixed solvent of water and ethanol for hydrolysis, then adding the micro-nanostructured molybdenum disulfide, stirring, washing, centrifuging and drying to obtain modified molybdenum disulfide; S2. Preparation of a hydrophobic anti-icing coating: After dissolving polydimethylsiloxane in an organic solvent, add the modified molybdenum disulfide obtained in step S1, and mix well to obtain the hydrophobic anti-icing coating based on molybdenum disulfide.

5. A method for preparing a hydrophobic anti-icing coating based on molybdenum disulfide as claimed in claim 4, characterized in that: In the step S1, the mass ratio of γ-aminopropyltriethoxysilane, water, ethanol and micro-nanostructured molybdenum disulfide is (0.8-1.2):1:(15-20):(0.3-0.7); and / or The hydrolysis time is 8 min to 12 min; and / or The stirring is magnetic stirring, and the stirring time is 1.5h to 2.5h; and / or The washing is performed using ethanol.

6. A method for preparing a hydrophobic anti-icing coating based on molybdenum disulfide as claimed in claim 4, characterized in that: In the step S2, the mass ratio of the modified molybdenum disulfide, polydimethylsiloxane and organic solvent is (15-35):(20-30):(800-1000); and / or The mixing operation is to perform ultrasonic treatment for 20 min to 40 min.

7. A hydrophobic anti-icing coating based on molybdenum disulfide, characterized in that: The coating is prepared by the preparation method of a hydrophobic anti-icing coating based on molybdenum disulfide as described in any one of claims 4 to 6.

8. An application of a hydrophobic anti-icing coating based on molybdenum disulfide, characterized in that: The molybdenum disulfide hydrophobic anti-icing coating prepared by the preparation method of a molybdenum disulfide hydrophobic anti-icing coating according to any one of claims 4 to 6 is sprayed on the surface of a substrate, and after drying and curing, a molybdenum disulfide hydrophobic anti-icing coating is obtained.

9. The use of a hydrophobic anti-icing coating based on molybdenum disulfide as claimed in claim 8, characterized in that: The spraying pressure is 3MPa to 5MPa; and / or The drying and curing temperature is 75° C. to 85° C., and the drying and curing time is 1.5 h to 2.2 h.

10. The use of a hydrophobic anti-icing coating based on molybdenum disulfide as claimed in claim 8, characterized in that: The substrate includes a metal substrate or a non-metal substrate; When the substrate is a metal substrate, the surface of the metal substrate is pretreated and then sprayed with the molybdenum disulfide-based hydrophobic anti-icing coating; The method for surface pretreatment of a metal substrate comprises the following steps: polishing the surface of the metal substrate with sandpaper, then ultrasonically washing it with ethanol and acetone in sequence, drying it, and then immersing the metal substrate in a mixed solution formed by mixing a dopamine hydrochloride solution and a Tris-HCl buffer solution to precipitate dopamine on the surface of the metal substrate, thereby completing the surface pretreatment of the metal substrate.

Citation Information

Cited By

  • Anti-icing coating, functional layer, multifunctional coating, preparation method and application

    CN120842987A