Gradient acid leaching-roasting method for recovering high-abundance valuable metal from red mud

High-abundance Ca, Al, Fe, and Na elements are separated from red mud through the stepped acid leaching and roasting method, which solves the problems of unreasonable design of separation steps and high energy consumption in the existing technology, and achieves efficient and economical multi-purpose Element separation and production of high-purity products provide a high-value utilization approach for red mud.

CN118724073APending Publication Date: 2024-10-01QUFU NORMAL UNIV

Patent Information

Application Number
CN202410774685.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When the existing technology extracts high-abundance valuable metals from red mud, the separation step design is unreasonable, the separation efficiency is low, the acid solution is used in large quantities, the equipment requirements are high, the operation is complex and energy-consuming, and it is difficult to achieve a variety of Complete separation of elements and production of high-purity products.

Method used

Using the stepwise acid leaching-roasting method, hydrochloric acid or industrial waste acid reacts with red mud to separate and obtain oxides containing calcium, aluminum and iron. Alkali and carbon dioxide are used to adjust the pH, and precipitation and roasting are performed to obtain CaCO3, Al2O3 and Fe2O3. Finally, through Sodium salt is obtained through evaporation and crystallization, achieving complete separation and efficient recovery of each element.

Benefits of technology

It achieves the efficient separation of high-abundance valuable elements in red mud and the preparation of pure products, reduces raw material costs, avoids high-temperature and high-pressure environments, the process is simple and economical, and no wastewater is generated, providing high-value utilization of low-value resources. way.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724073A_ABST
    Figure CN118724073A_ABST
Patent Text Reader

Abstract

The invention discloses an echelon acid leaching-roasting method for recovering high-abundance valuable metals from red mud, which comprises the following steps: (1) extracting Ca element in the red mud through an acid solution (hydrochloric acid or industrial waste acid) to obtain a calcium-containing solution and calcium-free red mud I, adding a precipitator into the calcium-containing solution, and introducing industrial waste gas CO2 to obtain calcium carbonate and a sodium salt solution I; (2) leaching the calcium-free red mud I with an acid solution to obtain an aluminum-containing solution and an iron-containing solid, and then precipitating or roasting to obtain aluminum oxide, iron oxide and a sodium salt solution II; and (3) mixing the sodium salt solution I with the sodium salt solution II, and performing evaporative crystallization to obtain the sodium salt. The method is low in raw material cost, simple in process, economical, green and low in energy consumption, efficient recovery of high-abundance valuable elements Ca, Al, Fe and Na in the red mud is achieved, functionalization of all the valuable metal elements is achieved, and high-valued collaborative comprehensive utilization of two low-value resources of industrial waste acid and industrial solid waste red mud is achieved through the thought of treating waste with waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal recovery, in particular to a cascade acid leaching-roasting method for recovering high-abundance valuable metals from red mud. Background Art

[0002] Red mud is a strong alkaline solid waste residue produced as a byproduct of aluminum oxide extraction in the aluminum industry. Its output has increased significantly with the rapid increase in market demand for aluminum. Red mud is mainly composed of compounds containing high-abundance elements such as Al, Fe, Si, Ti and trace elements such as Ni, Cd, K, Pb, etc. It is a precious and abundant secondary resource. Therefore, high value-added utilization of valuable elements in it has become an important research direction.

[0003] Chinese patent CN112095009A discloses a process for recovering calcium, sodium, aluminum, iron and rare earth chlorides from red mud by leaching red mud with hydrochloric acid. Although this method achieves the enrichment of calcium, sodium, aluminum, iron and rare earth chlorides by sequentially adding acid to red mud through three leaching devices, it only obtains a mixed solution containing multiple metal ions. However, this method cannot achieve the complete separation of related elements in red mud, and does not obtain corresponding pure metal oxides or compounds.

[0004] As we all know, due to the strong alkalinity and complex composition of red mud, it is extremely difficult to efficiently extract the valuable elements in red mud and completely separate them from each other. This has largely become one of the fundamental reasons why there has been no substantial breakthrough in the utilization of red mud worldwide for many years.

[0005] Chinese patent CN101182601A discloses a method for extracting metallic scandium and titanium from red mud. The method extracts trace amounts of scandium and titanium in red mud by three acid leachings to obtain titanium oxide and scandium oxide products. However, a large amount of acid is used in the process, and the valuable elements calcium and sodium are removed after leaching as impurities without being separated. Therefore, the obvious defect of this method is that it fails to effectively extract and separate calcium and sodium, and further fails to obtain the corresponding pure functional oxides or compounds containing calcium and sodium. The efficient separation of valuable elements has always been the goal pursued by the chemical industry.

[0006] In the patent application number 201810329555.9, Luo Honglin and others invented a method for recovering valuable metals from red mud. This method effectively recovers iron, titanium, gallium, aluminum, and scandium from red mud by adding concentrated sulfuric acid and coke for roasting and magnetic separation. However, roasting and magnetic separation methods require high energy consumption, complex operations, and poor economic benefits. They ignore the effective separation of different valuable elements and their subsequent functional utilization, and it is difficult to obtain high-purity products.

[0007] In addition, Chinese patent CN103898330A discloses that the traditional static hydrothermal method is used to extract the aluminum element in the red mud in the preparation of active boehmite porous microspheres using red mud as raw material. However, the preparation process must undergo high temperature and high pressure hydrothermal method, which is relatively harsh, energy-intensive, and requires high purity of the drug. In addition, only the single aluminum element in the red mud is extracted, and the high-abundance valuable components are far from being fully utilized.

[0008] Chinese patent CN117448581A discloses enriching Al, Fe, and Ti valuable elements in red mud and preparing them as functional materials through a rotary hydrothermal method. However, this method must use a rotary hydrothermal method, and still needs to rely on a high temperature and high pressure reactor environment. The reaction conditions are relatively harsh, especially for the extraction of valuable elements in red mud with high Ca content. It is not suitable for subsequent high-quality recovery of Al, Fe, and Ti elements, and the use of high-concentration acid has high equipment requirements, complex operations, and high energy consumption.

[0009] The above process of extracting elements from red mud has the following defects:

[0010] (1) Only a single element can be extracted;

[0011] (2) The element separation step is not designed properly, resulting in low separation efficiency of multiple elements;

[0012] (3) A large amount of acid solution is used;

[0013] (4) The equipment requirements are high, the operation is complex, and the energy consumption is high. Summary of the invention

[0014] The purpose of the present invention is to provide a cascade acid leaching-roasting method for recovering high-abundance valuable metals from red mud, so as to solve the problems of unreasonable design of separation steps of multiple high-abundance elements in red mud and poor separation efficiency.

[0015] To achieve the above object, the present invention provides a cascade acid leaching-roasting method for recovering high-abundance valuable metals from red mud, comprising the following steps:

[0016] S01: mixing red mud with an acid solution, heating and stirring, and separating to obtain a Ca-containing solution and calcium-free red mud I;

[0017] S02: Add alkali to the calcium solution to adjust the pH, then introduce CO 2 Adjust pH, stir and separate to obtain CaCO 3 Solid and sodium salt solution I;

[0018] S03: mixing the acid solution with the calcium-free red mud I, heating and stirring, and separating to obtain solution A and solid A;

[0019] S04: washing the solid A, mixing the washing liquid into the solution A to obtain a solution B and a gray solid B, and precipitating and separating the solution B to obtain an Al-containing solution and a Fe-containing solid;

[0020] S05: Wash, dry and calcine the Fe-containing solid to obtain Fe 2 O 3 ;

[0021] S06: mixing the washing liquid after iron washing into the Al-containing solution, adding acid to adjust the pH, stirring and separating to obtain the aluminum-containing solid and the sodium salt solution II;

[0022] S07: directly calcining the aluminum-containing solid to obtain Al 2 O 3 ;

[0023] S08: Mix the sodium salt solution I and the sodium salt solution II, evaporate and crystallize to obtain Na salt.

[0024] Preferably, in step S01 and step S03, the acid solution is hydrochloric acid or industrial hydrochloric acid. Industrial hydrochloric acid is industrial waste acid produced in large quantities in the metallurgical, electroplating, pharmaceutical and chemical industries, with a concentration of 30%-36% and containing Fe 2+ , Fe 3+ Ionic impurities.

[0025] In step S01, hydrochloric acid with a concentration of 0.1-2.0 mol / L or industrial hydrochloric acid with a dilution multiple of 5-35 times is used, the solid-liquid ratio of red mud to acid solution is 1:10-1:40, the heating temperature is 40-80°C, and the stirring time is 1.0-4.0h;

[0026] In step S03, hydrochloric acid with a concentration of 3-12 mol / L or untreated industrial hydrochloric acid is used, the solid-liquid ratio of calcium-free red mud I to the acid solution is 1:10-1:40, the heating temperature is 90-120° C., and the stirring time is 0.5-4.0 h.

[0027] Preferably, in step S01, the concentration of hydrochloric acid is 0.2-1.5 mol / L, the dilution multiple of industrial hydrochloric acid is 7-30 times, the solid-liquid ratio of red mud to acid solution is 1:10-1:30, the heating temperature is 50-70°C, and the stirring time is 1.5-3.5h.

[0028] Preferably, in step S03, the solid-liquid ratio of the calcium-free red mud I to the acid solution is 1:20-1:30, the heating temperature is 100° C., and the stirring time is 1.0-3.5 h.

[0029] Preferably, in step S02, the base is 2-6 mol / L sodium hydroxide, the base is added to adjust the pH to 10-13, and CO is introduced 2Adjust the pH to 6-9 and the stirring time to 1.0-6.0h.

[0030] Preferably, in step S02, the concentration of sodium hydroxide is 3-5 mol / L, the pH is adjusted to 10.5-12.5, and CO is introduced. 2 Adjust the pH to 6-8 and the stirring time to 2.0-5.0h.

[0031] Preferably, in step S02, the yield of Ca element extracted from red mud is 70-99%.

[0032] Preferably, in step S04, solid A is washed with deionized water until it turns gray.

[0033] Preferably, in step S04, a 3-7 mol / L NaOH solution is added dropwise to solution B without generating red precipitate, and after stirring for 0.5-6.0 h, the Al-containing solution and the Fe-containing solid are separated by centrifugation or suction filtration. More preferably, the concentration of the NaOH solution is 4-6 mol / L, and the stirring time is 1.0-5.0 h.

[0034] Preferably, in step S05, the Fe-containing solid is washed with deionized water to neutrality; the drying temperature is 50-100°C and the time is 6.0-12.0h; the roasting temperature is 600-1000°C and the roasting time is 4.0-8.0h.

[0035] More preferably, in step S05, the drying temperature is 60-80°C, the drying time is 8.0-10.0 hours, the roasting temperature is 700-900°C, and the roasting time is 2.0-6.0 hours.

[0036] Preferably, in step S05, the yield of Fe element extracted from red mud is 60-99%.

[0037] Preferably, in step S06, the acid added is 0.1-3.0 mol / L of acidic liquid or acidic gas CO 2 The acidic liquid is one of hydrochloric acid or nitric acid.

[0038] Preferably, in step S06, when an acidic liquid is used, the pH is adjusted to 4-9, and the stirring time is 0.5-4.0 h; when an acidic gas is used, the pH is adjusted to 11-8, and the stirring time is 2.0-8.0 h.

[0039] More preferably, in step S06, when an acidic liquid is used, the concentration is 0.1-1.5 mol / L, the pH is 8.5-4.5, and the stirring time is 0.5-3.5 h; when an acidic gas is used, the pH is 10.5-8.5, and the stirring time is 4.0-8.0 h.

[0040] Preferably, in step S07, the calcination temperature is 600-1100° C., and the calcination time is 2.0-6.0 h.

[0041] More preferably, in step S07, the calcination temperature is 700-1000° C., and the calcination time is 2.0-4.0 h.

[0042] Preferably, in step S07, the yield of Al element extracted from red mud is 70-99%.

[0043] Preferably, in step S08, sodium salt solution I and sodium salt solution II are first mixed;

[0044] When hydrochloric acid is used in step S06, the evaporative crystallization is to directly evaporate at 60-100° C. to obtain NaCl;

[0045] When nitric acid is used in step S06, the evaporation crystallization is to first use silver nitrate with a concentration of 0.1-1.0 mol / L to react with NaCl in a sodium salt solution to generate precipitated AgCl, and then evaporate the filtrate at 60-100°C to obtain NaNO 3 ;

[0046] In step S06, the acid gas CO is used 2 The evaporation crystallization is to first use calcium chloride with a concentration of 0.1-1.0 mol / L to react with sodium carbonate in the sodium salt to generate a precipitate CaCO 3 After separation, the filtrate is evaporated at 60-100°C to obtain NaCl.

[0047] More preferably, in step S06, the evaporation temperature is 60-90°C.

[0048] It should be noted that the method for calculating the element yield in steps S02, S05 and S07 is: the element content in the red mud is obtained by inductively coupled plasma mass spectrometry (ICP-MS), the element mass of the red mud is calculated, and then the element yield of the product can be obtained by calculating the elements in the product.

[0049] Therefore, the present invention adopts a cascade acid leaching-roasting method for recovering high-abundance valuable metals from red mud with the above structure, which has the following beneficial effects:

[0050] (1) The present invention firstly uses hydrochloric acid or industrial waste acid (industrial hydrochloric acid) to accurately and simply leach the high-abundance valuable component Ca in red mud, then adds a precipitant and introduces CO 2 The calcium-containing product CaCO 3 Secondly, hydrochloric acid or industrial hydrochloric acid is used to extract the high-abundance valuable components Al and Fe in the calcium-free red mud after calcium extraction, and the waste liquid generated by washing is recycled and reused. The corresponding product Al is obtained by simple precipitation and roasting methods. 2O 3 and Fe 2 O 3 , achieving efficient recovery of Al and Fe elements. The final wastewater is mainly a neutral salt solution, which can be evaporated and crystallized to obtain the corresponding sodium salt. The Na in the red mud is separated and recovered, achieving zero discharge of process wastewater.

[0051] (2) The acid solution of the present invention can utilize industrial waste acid (industrial hydrochloric acid) to efficiently extract and enrich the high-abundance valuable elements Ca, Al, Fe, and Na in red mud through cascade acid leaching, and then obtain the product CaCO through mild and simple precipitation-roasting. 3 、Al 2 O 3 and Fe 2 O 3 , Na salt is obtained by evaporation and crystallization, which can be sold directly, or supplied back to alumina plants, or supplied to aluminum flocculant plants, or supplied to steel mills and other enterprises to fully improve quality and efficiency.

[0052] (3) Compared with the prior art that uses analytically pure hydrochloric acid to enrich the corresponding metal elements from red mud as a whole but fails to achieve complete separation of the metal elements from each other, the present invention cleverly uses dilute hydrochloric acid or industrial waste acid to treat red mud, achieves the step-by-step leaching of high-abundance valuable elements from red mud, accurately controls the complete separation of the elements from each other, and obtains pure functional oxides or compounds of the elements. This idea has not been publicly reported so far, and the raw material cost is significantly low, the process does not require a high temperature and high pressure environment, is simple, economical and green, has a high recovery rate, does not generate wastewater, and is easy to scale up by pilot testing. When using waste acid, it also provides a new idea of ​​"treating waste with waste" for the high-value utilization of two low-value resources, industrial waste acid and bulk solid waste red mud.

[0053] (4) The process of the present invention is highly universal for efficiently extracting high-abundance valuable elements Ca, Al, Fe, and Na from red mud of different compositions in different regions (especially red mud with high aluminum, high iron, and high calcium content), achieving complete separation and functionalization of the elements.

[0054] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 is a process flow chart of the present invention;

[0056] Figure 2 is CaCO in Example 1 3 XRD spectrum of

[0057] Figure 3 is Fe in Example 1 2 O 3XRD spectrum of

[0058] Figure 4 is Al in Example 1 2 O 3 XRD spectrum of . DETAILED DESCRIPTION

[0059] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment.

[0060] Example 1

[0061] A cascade acid leaching-roasting method for efficiently recovering high-abundance valuable metals from red mud, the method comprising:

[0062] S101: Red mud was mixed with 0.2 mol / L hydrochloric acid at a solid-liquid ratio of 1:10, heated to 50°C, stirred for 1.5 hours, and then filtered to separate the calcium-containing solution and calcium-free red mud I.

[0063] S102: Add 3 mol / L sodium hydroxide to the calcium solution, adjust the pH to 11, and then introduce CO 2 Adjust the pH to 8, stir for 2.0 h, and separate the sodium salt solution I and the calcium extraction product CaCO 3 The calcium extraction rate was 98.5%.

[0064] S103: industrial hydrochloric acid was mixed with calcium-free red mud I at a solid-liquid ratio of 1:10, heated to 100° C., stirred for 1.0 h to obtain a reaction mixture, and solution A and solid A were separated by suction filtration.

[0065] S104: Wash solid A with deionized water until the color changes to gray, and recycle the washing liquid and mix it into solution A in S103 to obtain solution B. Then, add 4.0 mol / L NaOH solution dropwise to solution B until no red precipitate is produced. After stirring for 1.0 h, separate the Al-containing solution and the Fe-containing solid by suction filtration.

[0066] S105: The Fe-containing solid is washed with deionized water until it is neutral, dried at 60°C for 8.0 hours, and then placed in a tube furnace and calcined at 800°C in an air atmosphere for 4.0 hours to obtain the red mud Fe extraction product Fe 2 O 3 The yield of Fe element is 72.9%.

[0067] S106: The washing liquid after iron washing is mixed into the Al-containing solution, and the pH is adjusted to 8.5 by using 0.1 mol / L hydrochloric acid. After stirring for 0.5 h, the aluminum-containing solid and the sodium salt solution II are separated by centrifugation or suction filtration.

[0068] S107: The aluminum-containing solid is placed in a tube furnace and calcined at 1000°C in an air atmosphere for 2 hours to obtain the red mud Al extraction product Al 2 O 3 The Al element yield was 98.7%.

[0069] S108: Mix the sodium salt solution I and the sodium salt solution II and evaporate them directly at 60° C. to obtain NaCl.

[0070] Example 2

[0071] A cascade acid leaching-roasting method for efficiently recovering high-abundance valuable metals from red mud, the method comprising:

[0072] S201: Red mud was mixed with 1.5 mol / L hydrochloric acid at a solid-liquid ratio of 1:15, heated to 60°C, stirred for 2.0 h, and then filtered to separate the calcium-containing solution and calcium-free red mud I.

[0073] S202: Add 4 mol / L sodium hydroxide to the calcium solution, adjust the pH to 11.5, and then introduce CO 2 The pH was adjusted to 7 and stirred for 3.0 h to separate the sodium salt solution I and the calcium extraction product CaCO. 3 The calcium extraction rate was 97.1%.

[0074] S203: 3 mol / L hydrochloric acid was mixed with calcium-free red mud I at a solid-liquid ratio of 1:15, heated to 100° C., stirred for 1.5 h to obtain a reaction mixture, and solution A and solid A were separated by suction filtration.

[0075] S204: Wash solid A with deionized water until the color turns gray, and recycle the washing liquid and mix it into solution A in S203 to obtain solution B. Then, add 5.0 mol / L NaOH solution dropwise to solution B until no red precipitate is produced, stir for 1.5 hours, and separate by suction filtration to obtain Al-containing solution and Fe-containing solid.

[0076] S205: The Fe-containing solid was washed with deionized water until it was neutral, and dried at 70°C for 8.0 hours. Then, it was placed in a tube furnace and calcined at 700°C in an air atmosphere for 4.0 hours to obtain the red mud Fe extraction product Fe 2 O 3 The yield of Fe element is 98.2%.

[0077] S206: The washing liquid after iron washing is mixed into the Al-containing solution, and the pH is adjusted to 4.5 by using 0.5 mol / L hydrochloric acid. After stirring for 1.0 h, the aluminum-containing solid and the sodium salt solution II are separated by centrifugation or suction filtration.

[0078] S207: The aluminum-containing solid is placed in a tube furnace and calcined at 700°C in an air atmosphere for 2 hours to obtain the red mud Al extraction product Al 2 O 3 The Al element yield was 60.2%.

[0079] S208: Mix the sodium salt solution I and the sodium salt solution II and evaporate them at 70° C. to obtain NaCl.

[0080] Example 3

[0081] A cascade acid leaching-roasting method for efficiently recovering high-abundance valuable metals from red mud, the method comprising:

[0082] S301: Mix red mud with industrial hydrochloric acid diluted 12 times at a solid-liquid ratio of 1:20, heat to 70°C, stir for 2.0 hours, and then filter and separate to obtain a calcium-containing solution and calcium-free red mud I.

[0083] S302: Add 4 mol / L sodium hydroxide to the calcium solution, adjust the pH to 12, and then introduce CO 2 The pH was adjusted to 7 and stirred for 3.5 h to separate the sodium salt solution I and the calcium extraction product CaCO. 3 The calcium extraction rate was 96.8%.

[0084] S303: 12 mol / L hydrochloric acid was mixed with calcium-free red mud I at a solid-liquid ratio of 1:20, heated to 110° C., stirred for 2.0 h to obtain a reaction mixture, and solution A and solid A were separated by suction filtration.

[0085] S304: Solid A is washed with deionized water until the color turns gray, and the washing liquid is recovered and mixed into solution A in S303 to obtain solution B. 6 mol / L NaOH solution is then added dropwise to solution B until no red precipitate is produced. After stirring for 2.0 h, the Al-containing solution and the Fe-containing solid are separated by suction filtration.

[0086] S305: The Fe-containing solid is washed with deionized water until it is neutral, and dried at 90°C for 10.0h. Then, it is placed in a tube furnace and calcined at 900°C in an air atmosphere for 4.0h to obtain the red mud Fe extraction product Fe 2 O 3 The yield of Fe element is 98.9%.

[0087] S306: The washing liquid after iron washing is mixed into the Al-containing solution, and the pH is adjusted to 8.0 by using 1 mol / L nitric acid. After stirring for 1.5 hours, the aluminum-containing solid and the sodium salt solution II are separated by centrifugation or suction filtration.

[0088] S307: The aluminum-containing solid is placed in a tube furnace and calcined at 800°C in an air atmosphere for 4 hours to obtain the red mud Al extraction product Al 2 O 3 The Al element yield was 97.3%.

[0089] S308: After mixing sodium salt solution I and sodium salt solution II, a silver nitrate solution with a concentration of 0.1 mol / L is used to react with the NaCl in the mixed sodium salt solution to generate precipitated AgCl. After separation, the filtrate is evaporated at 70°C to obtain NaNO 3 .

[0090] Example 4

[0091] A cascade acid leaching-roasting method for efficiently recovering high-abundance valuable metals from red mud, the method comprising:

[0092] S401: Mix red mud with industrial hydrochloric acid diluted 30 times at a solid-liquid ratio of 1:25, heat to 70°C, stir for 3.0 hours, and then filter and separate to obtain a calcium-containing solution and calcium-free red mud I.

[0093] S402: Add 6 mol / L sodium hydroxide to the calcium solution, adjust the pH to 12.5, and then introduce CO 2 The pH was adjusted to 7 and stirred for 4.0 h to separate the sodium salt solution I and the calcium extraction product CaCO. 3 The calcium extraction rate was 97.5%.

[0094] S403: industrial hydrochloric acid was mixed with calcium-free red mud I at a solid-liquid ratio of 1:25, heated to 110° C., stirred for 2.5 h to obtain a reaction mixture, and solution A and solid A were separated by suction filtration.

[0095] S404: Wash solid A with deionized water until the color turns gray, and recover the washing liquid and mix it into solution A in S403 to obtain solution B. Then, add 6 mol / L NaOH solution dropwise to solution B until no red precipitate is produced. After stirring for 2.5 h, separate the Al-containing solution and the Fe-containing solid by suction filtration.

[0096] S405: The Fe-containing solid is washed with deionized water until it is neutral, and dried at 80°C for 8.0 hours. Then, it is placed in a tube furnace and calcined at 800°C in an air atmosphere for 4.0 hours to obtain the red mud Fe extraction product Fe 2 O3 The yield of Fe element is 96.3%.

[0097] S406: Mix the iron washing solution into the Al-containing solution and introduce CO 2 The pH value was adjusted to 10.5, and after stirring for 4.0 hours, the aluminum-containing solid and the sodium salt solution II were separated by centrifugation or suction filtration.

[0098] S407: The aluminum-containing solid is placed in a tube furnace and calcined at 850°C in an air atmosphere for 4 hours to obtain the red mud Al extraction product Al 2 O 3 The Al element yield was 67.3%.

[0099] S408: After the sodium salt solution I and the sodium salt solution II are mixed, a 0.1 mol / L calcium chloride solution is first used to react with the sodium carbonate in the mixed sodium salt solution to generate precipitated calcium carbonate, and after separation, the filtrate is evaporated at 80° C. to obtain NaCl.

[0100] Example 5

[0101] A cascade acid leaching-roasting method for efficiently recovering high-abundance valuable metals from red mud, the method comprising:

[0102] S501: Mix red mud with industrial hydrochloric acid diluted 30 times at a solid-liquid ratio of 1:25, heat to 75°C, stir for 3.5 hours, and then filter and separate to obtain a calcium-containing solution and calcium-free red mud I.

[0103] S502: Add 6 mol / L sodium hydroxide to the calcium solution, adjust the pH to 13.0, and then introduce CO 2 The pH was adjusted to 6 and stirred for 5.0 h to separate the sodium salt solution I and the calcium extraction product CaCO. 3 The calcium extraction rate was 98.9%.

[0104] S503: Use industrial hydrochloric acid to mix with red mud at a solid-liquid ratio of 1:30, heat to 110° C., stir for 3.0 hours to obtain a reaction mixture, and separate by suction filtration to obtain solution A and solid A.

[0105] S504: Solid A is washed with deionized water until the color changes to gray, and the washing liquid is recovered and mixed into solution A in S503 to obtain solution B. Then, 6 mol / L NaOH solution is added dropwise to solution B until no red precipitate is produced. After stirring for 3.0 h, Al-containing solution and Fe-containing solid are separated by suction filtration.

[0106] S505: The Fe-containing solid is washed with deionized water until it is neutral, and dried at 80°C for 8.0 hours. Then, it is placed in a tube furnace and calcined at 800°C in an air atmosphere for 4.0 hours to obtain the red mud Fe extraction product Fe 2 O 3 The yield of Fe element is 96.3%.

[0107] S506: Mix the washing liquid after iron washing into the Al-containing solution, and introduce CO 2 The pH value was adjusted to 8.5, and after stirring for 6.0 hours, the aluminum-containing solid and the sodium salt solution II were separated by centrifugation or suction filtration.

[0108] S507: The aluminum-containing solid is placed in a tube furnace and calcined at 900°C in an air atmosphere for 4 hours to obtain the red mud Al extraction product Al 2 O 3 The Al element yield was 73.8%.

[0109] S508: After the sodium salt solution I and the sodium salt solution II are mixed, a 0.5 mol / L calcium chloride solution is first used to react with the sodium carbonate in the mixed sodium salt solution to generate precipitated calcium carbonate, and after separation, the filtrate is evaporated at 80° C. to obtain NaCl.

[0110] The yields of various elements in Examples 1-5 are shown in Table 1.

[0111] Table 1 Yield of each element in Examples 1-5

[0112]

[0113] Therefore, the present invention adopts a cascade acid leaching-roasting method of the above structure to recover high-abundance valuable metals from red mud, uses hydrochloric acid or industrial waste acid for leaching and extracts high-abundance Ca, Al, Fe, and Na elements in red mud through a simple process, has a high element yield and no waste liquid output, and provides a green, economical and effective method for treating red mud.

[0114] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A cascade acid leaching-roasting method for recovering high-abundance valuable metals from red mud, characterized in that: The following steps are involved: S01: mixing red mud with an acid solution, heating and stirring, and separating to obtain a Ca-containing solution and calcium-free red mud I; S02: adding alkali to the calcium-containing solution to adjust the pH, then introducing CO2 to adjust the pH, stirring and separating to obtain CaCO3 solid and sodium salt solution I; S03: mixing the acid solution with the calcium-free red mud I, heating and stirring, and separating to obtain solution A and solid A; S04: washing the solid A, mixing the washing liquid into the solution A to obtain a solution B and a gray solid B, and precipitating and separating the solution B to obtain an Al-containing solution and a Fe-containing solid; S05: washing, drying and calcining the Fe-containing solid to obtain Fe2O3; S06: mixing the washing liquid after iron washing into the Al-containing solution, adding acid to adjust the pH, stirring and separating to obtain the aluminum-containing solid and the sodium salt solution II; S07: directly calcining the aluminum-containing solid to obtain Al2O3; S08: Mix the sodium salt solution I and the sodium salt solution II, evaporate and crystallize to obtain Na salt.

2. The method of claim 1 for recovering high-abundance valuable metals from red mud by cascade acid leaching and roasting, characterized in that: In step S01 and step S03, the acid solution is one of hydrochloric acid or industrial hydrochloric acid; In step S01, hydrochloric acid with a concentration of 0.1-2.0 mol / L or industrial hydrochloric acid with a dilution multiple of 5-35 times is used, the solid-liquid ratio of red mud to acid solution is 1:10-1:40, the heating temperature is 40-80°C, and the stirring time is 1.0-4.0h; In step S03, hydrochloric acid with a concentration of 3-12 mol / L or untreated industrial hydrochloric acid is used, the solid-liquid ratio of calcium-free red mud I to the acid solution is 1:10-1:40, the heating temperature is 90-120° C., and the stirring time is 0.5-4.0 h.

3. The method of claim 1 for recovering high-abundance valuable metals from red mud by cascade acid leaching and roasting, characterized in that: In step S02, the alkali is 2-6 mol / L sodium hydroxide, the alkali is added to adjust the pH to 10-13, CO2 is introduced to adjust the pH to 6-9, and the stirring time is 1.0-6.0 h.

4. The method of claim 1 for recovering high-abundance valuable metals from red mud by cascade acid leaching and roasting, characterized in that: In step S04, the solid A is washed with deionized water until it turns gray.

5. The method of claim 1 for recovering high-abundance valuable metals from red mud by cascade acid leaching and roasting, characterized in that: In step S05, the Fe-containing solid is washed with deionized water to neutrality; the drying temperature is 50-100°C and the time is 6.0-12.0 hours; the roasting temperature is 600-1000°C and the roasting time is 4.0-8.0 hours.

6. The method of claim 1 for recovering high-abundance valuable metals from red mud by cascade acid leaching and roasting, characterized in that: In step S06, the added acid is one of 0.1-3.0 mol / L acidic liquid or acidic gas CO2, and the acidic liquid is one of hydrochloric acid or nitric acid.

7. The method of claim 6 for recovering high-abundance valuable metals from red mud by cascade acid leaching and roasting, characterized in that: In step S06, when an acidic liquid is used, the pH is adjusted to 4-9 and the stirring time is 0.5-4.0 hours; when an acidic gas is used, the pH is adjusted to 11-8 and the stirring time is 2.0-8.0 hours.

8. The method of claim 1 for recovering high-abundance valuable metals from red mud by cascade acid leaching and roasting, characterized in that: In step S07, the calcination temperature is 600-1100° C., and the calcination time is 2.0-6.0 h.

9. The method of claim 7 for recovering high-abundance valuable metals from red mud by cascade acid leaching and roasting, characterized in that: In step S08, sodium salt solution I and sodium salt solution II are first mixed; When hydrochloric acid is used in step S06, the evaporative crystallization is to directly evaporate at 60-100° C. to obtain NaCl; When nitric acid is used in step S06, the evaporation crystallization is to first use silver nitrate with a concentration of 0.1-1.0 mol / L to react with NaCl in a sodium salt solution to generate precipitated AgCl, and then evaporate the filtrate at 60-100° C. to obtain NaNO3 after separation; When acidic gas CO2 is used in step S06, the evaporation crystallization is to first use calcium chloride with a concentration of 0.1-1.0 mol / L to react with sodium carbonate in the sodium salt to generate precipitated CaCO3, and after separation, evaporate the filtrate at 60-100°C to obtain NaCl.

Citation Information

Patent Citations

  • Method for extracting metal scandium and titanium from red mud

    CN101182601A

  • Method for comprehensively recycling such valuable metals as iron, aluminum, scandium, titanium, vanadium and the like in red mud

    CN103898330A

  • Recovery method of red mud

    CN108384956A

  • Process for recovering chlorides of calcium, sodium, aluminum, iron and rare earth by leaching red mud by using hydrochloric acid

    CN112095009A

  • Rotation hydrothermal method for preparing functional oxide by extracting valuable metal from red mud, constructed composite membrane and application of composite membrane

    CN117448581A

Cited By

  • Method for converting red mud into mineral resources

    CN120362234A