A treatment process for enriching and recovering nickel from lithium battery industrial wastewater
Through the process of modifying biochar to form complex precipitation and conversion of tetracarbonyl nickel, the problem of difficulty in separation of nickel and cobalt in lithium battery wastewater is solved, and the efficient recycling and resource utilization of nickel is achieved.
Patent Information
- Application Number
- CN202410823214.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-06-25
AI Technical Summary
It is difficult to separate nickel and cobalt in the industrial wastewater of lithium batteries, and there are difficulties in the existing extraction methods, and the recycling efficiency of nickel is low, so efficient enrichment and recycling processes are needed.
The suspension and organic matter were removed by pre-filtration, and a stable complex precipitation was formed using modified biochar. The nickel ions were then converted into gaseous tetracarbonyl nickel and separated. The recovery of nickel and the distinction from cobalt were achieved in combination with various processes.
The efficient enrichment and recovery rate of nickel is achieved to reach more than 95%, effectively distinguishing nickel and cobalt, improving resource utilization efficiency, and avoiding adverse effects of subsequent processes.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy industrial wastewater treatment, and in particular to a treatment process for enriching and recovering nickel from lithium battery industrial wastewater. Background Art
[0002] With the rapid development of the new energy industry, lithium batteries, as a kind of energy storage element, have also expanded their production capacity and application in the fields of new energy vehicles. The production process of lithium batteries will produce wastewater, mainly including positive electrode wastewater and negative electrode wastewater, which are complex in composition, poor in biodegradability, and contain heavy metals and toxic substances. They need to be treated before they can be discharged to the downstream sewage treatment plant. Positive electrode wastewater mainly contains inorganic salts, heavy metal ions (such as nickel, cobalt, manganese, etc.) and organic additives. Negative electrode wastewater mainly contains common COD (chemical oxygen demand), SS (suspended solids) and a small amount of metal ions (such as copper, iron, etc.) and organic solvents. In view of the large difference between positive and negative electrode wastewater, and the high recovery value of heavy metal ions in positive electrode wastewater, resource utilization can be achieved through appropriate treatment processes. Therefore, it is more reasonable to polarize the treatment of positive and negative electrode wastewater, and recycle as much as possible.
[0003] Nickel is an important metal resource, widely used in alloy materials and batteries. With the acceleration of global industrialization, the demand for these materials is growing, which has promoted the development of the nickel scrap market. The cost of recovering nickel is usually lower than the cost of mining primary nickel ore, so it is economically valuable to recover nickel from lithium battery industrial wastewater. Since cobalt and nickel have similar properties, including similar physical properties and similar chemical properties, there are certain difficulties in their separation process. At present, lithium battery industrial wastewater usually uses extraction method to selectively extract nickel and cobalt, and there is a need for a recovery method that enriches nickel. Summary of the invention
[0004] In order to solve the problems mentioned in the background technology, the present invention provides a treatment process for enriching and recovering nickel from lithium battery industrial wastewater, which first removes suspended solids and organic matter in the wastewater to avoid adverse effects on subsequent processes, and then constructs modified biochar to utilize its ability to form stable complex precipitation with nickel ions and its large specific surface area to achieve nickel ion enrichment, and then through a series of coordinated processes, the nickel ions are converted into gaseous tetracarbonyl nickel and separated from the system, thereby achieving nickel recovery and effectively separating it from cobalt.
[0005] Specifically:
[0006] A treatment process for enriching and recovering nickel from lithium battery industrial wastewater, the steps of which include:
[0007] Step 1: pre-filter the lithium battery industrial wastewater to obtain filtrate A; remove large suspended particles in the wastewater, such as plastic fragments, metal particles, etc.;
[0008] Step 2: adjust the pH value of the A filtrate to 7-7.5, add a coagulant and stir, stop stirring to allow the coagulated particles to settle to the bottom, separate the upper liquid and pass it through an activated carbon filter; according to the pH value of the wastewater, use acid or alkali to adjust it to a neutral or alkaline range to promote the removal of organic matter in the subsequent treatment process; adding a coagulant can make the suspended particles and organic matter condense into larger particles and settle at the bottom; the activated carbon filter further removes suspended particles, fine coagulants, and organic matter in the wastewater;
[0009] Step 3, adding a precipitant to the upper layer liquid, controlling the pH value at 7-8, filtering after the precipitation is complete, and obtaining filtrate B; precipitating most metal ions such as calcium, manganese, iron, magnesium, aluminum, etc.;
[0010] Step 4: Add modified biochar into the filtrate B, filter after the reaction is completed, and collect the filtered modified biochar; the modified biochar used is surface-modified with potassium permanganate and potassium hydroxide;
[0011] Step 5, drying the filtered modified biochar and placing it in a hydrogen reduction furnace filled with hydrogen for reduction, and taking out the reduced modified biochar after the reaction is completed;
[0012] Step 6: ball-mill the reduced modified biochar, then put it into a reaction container, add carbon monoxide, control the temperature at 45-55°C for full reaction, exhaust the gas under insulation conditions after the reaction, and cool and condense the exhaust gas to obtain nickel tetracarbonyl liquid;
[0013] Step 7: thermally decompose the tetracarbon-based nickel to obtain metallic nickel.
[0014] When implementing the above embodiment, preferably, step 1 uses a coarse filter or a grid as a pre-filter.
[0015] When implementing the above embodiment, preferably, in step 2, the coagulant is polyaluminum chloride or polyferric sulfate, and the amount of coagulant added is 1-5 g / L; the stirring time is 5-10 minutes; the sedimentation time is 1-4 hours; the amount of activated carbon added to the activated carbon filter is 5-100 g / L, and the filtration speed is 5-10 m / h.
[0016] When implementing the above embodiment, preferably, in step 3, the precipitant is sodium hydroxide; and the precipitation time is 0.5-2h.
[0017] When implementing the above embodiment, preferably, the input amount of modified biochar in step 4 is 0.5-2 g / L, and the reaction time is 3-6 h.
[0018] When implementing the above embodiment, preferably, the preparation process of the modified biochar in step 4 includes: carbonizing the biochar source at a high temperature of 500-600°C to obtain the biochar; immersing the biochar in a potassium permanganate solution with a concentration of 0.01-0.1 mol / L, and reacting for 0.5-1.5 hours; then taking out the biochar and immersing it in a potassium hydroxide solution with a concentration of 0.1-1 mol / L, reacting for 0.5-1 hour, and taking it out and drying it.
[0019] Furthermore, the biochar source is selected from a mixture of one or more of fruit husks, rice husks, straw, and sugarcane bagasse.
[0020] When implementing the above embodiment, preferably, in step 5, the temperature of the hydrogen reduction furnace is controlled at 200-400° C., and the pressure is controlled at 1-10 atm.
[0021] When implementing the above embodiment, preferably, in step 6, the modified biochar is ball-milled to 70-90 μm.
[0022] When implementing the above embodiment, preferably, the sufficient reaction time in step 6 is 0.5-1h; the temperature of the cooling and condensation is controlled at 20-25°C.
[0023] Compared with the prior art, the present invention has the following beneficial features:
[0024] 1. In the treatment process of the present invention, biochar modified by potassium permanganate and potassium hydroxide is added. The combined modification of potassium permanganate and potassium hydroxide can significantly improve the adsorption capacity of biochar for nickel ions. Stable complexes of nickel hydroxide and complex nickel oxide are formed by coprecipitation and complexation with nickel ions and precipitated and adsorbed on the surface of biochar. In addition, the surface of biochar has abundant porous skeletons with large specific surface area. The synergistic structure is used to efficiently enrich nickel ions and improve the nickel recovery rate, which is above 95%.
[0025] 2. In the treatment process of the present invention, the nickel ion complex precipitated on the modified biochar is reduced to active nickel by hydrogen under specific conditions, and then reacted with carbon monoxide to generate nickel tetracarbonyl, and the temperature is adjusted so that the nickel tetracarbonyl is discharged in gaseous form. The nickel element is separated from the system by the synergistic effect of multiple steps, thereby realizing the recovery of the nickel element; although the cobalt ions in the system will also be reduced to active cobalt during this period, they will not generate gaseous products with carbon monoxide, and cobalt has a certain catalytic effect, which will further improve the efficiency of converting active nickel into nickel tetracarbonyl.
[0026] 3. The treatment process of the present invention also pre-treats the wastewater to remove suspended solids and organic matter in the wastewater to avoid adverse effects on subsequent processes. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] In order to facilitate those skilled in the art to implement the present invention, some of the reagents used in the embodiments and comparative examples are now described:
[0029] Coagulant: polyferric sulfate, Gongyi Yiqing water purification materials;
[0030] Precipitant: sodium hydroxide, produced by Shanghai Shengfuze Chemicals;
[0031] Potassium permanganate: Zhengzhou Shuoyuan Biotechnology;
[0032] Potassium hydroxide: Jiangsu Leien Environmental Protection Technology;
[0033] Biochar source: rice husk, Guangxi Zhuangda Fertilizer Industry;
[0034] Hydrogen: 5N hydrogen, from Foshan Kedi Gas Chemical;
[0035] Carbon monoxide: 4N carbon monoxide, Jining Sanzheng Machinery Equipment;
[0036] Lithium battery industrial wastewater: Nickel-cobalt-manganese ternary lithium battery positive electrode wastewater is selected, and its components mainly contain nickel element concentration of 29 mg / L, cobalt element concentration of 41 mg / L, manganese element concentration of 22 mg / L, magnesium element concentration of 145 mg / L, COD concentration of 2800 mg / L, petroleum concentration of 47 / L, suspended matter concentration of 649 mg / L, and sulfate concentration of 34905 mg / L.
[0037] Example 1
[0038] A treatment process for enriching and recovering nickel from lithium battery industrial wastewater, treating 15,000L of nickel-cobalt-manganese ternary lithium battery positive electrode wastewater, the steps of which include:
[0039] Step 1: pre-filter lithium battery industrial wastewater using a grid to obtain filtrate A;
[0040] Step 2, adjusting the pH value of the A filtrate to 7, adding polyferric sulfate in an amount of 1 g / L according to the volume of the A filtrate, and stirring for 5 minutes, stopping stirring and waiting for the condensed particles to settle to the bottom, the sedimentation time is 1 hour, separating the upper layer liquid and passing it through an activated carbon filter, filling the activated carbon filter with activated carbon in an amount of 5 g / L according to the volume of the upper layer liquid, and the filtration speed is 10 m / h;
[0041] Step 3, adding sodium hydroxide to the upper layer liquid, the amount of sodium hydroxide added is 5 g / L, the pH value is controlled at 7, the precipitation time is 0.5 h, and after the precipitation is complete, filtering is performed to obtain filtrate B;
[0042] Step 4: Add modified biochar to the filtrate B, the amount of modified biochar added is 0.5 g / L, the reaction time is 3 h, filter after the reaction is completed, and collect the filtered modified biochar;
[0043] The modified biochar used is surface-modified with potassium permanganate and potassium hydroxide, and the steps include: carbonizing rice husks at 500°C to obtain biochar; immersing the biochar in a 0.01 mol / L potassium permanganate solution and reacting it for 0.5 h; then taking out the biochar and immersing it in a 0.1 mol / L potassium hydroxide solution and reacting it for 0.5 h, and then taking out and drying it.
[0044] Step 5, drying the filtered modified biochar and placing it in a hydrogen reduction furnace to fill it with hydrogen, the hydrogen flow rate is controlled at 30 ml / min, the temperature of the hydrogen reduction furnace is controlled at 200°C, and the pressure is controlled at 1-10 atm. After the reaction is completed, the reduced modified biochar is taken out;
[0045] Step 6, ball-mill the reduced modified biochar to 70 μm, then put it into a reaction container, add carbon monoxide, control the temperature at 45°C to fully react for 0.5 h, exhaust under insulation conditions after the reaction, and cool the exhaust gas to 20°C for condensation to obtain tetracarbonyl nickel liquid;
[0046] Step 7: thermally decompose the tetracarbon-based nickel to obtain metallic nickel.
[0047] The nickel recovery rate through the above method is 96.8%.
[0048] Example 2
[0049] A treatment process for enriching and recovering nickel from lithium battery industrial wastewater, treating 20,000L of nickel-cobalt-manganese ternary lithium battery positive electrode wastewater, the steps of which include:
[0050] Step 1: pre-filter lithium battery industrial wastewater using a grid to obtain filtrate A;
[0051] Step 2, adjusting the pH value of the A filtrate to 7.5, adding polyferric sulfate in an amount of 5 g / L according to the volume of the A filtrate, and stirring for 10 minutes, stopping stirring and waiting for the condensed particles to settle to the bottom, the sedimentation time is 4 hours, separating the upper layer liquid and passing it through an activated carbon filter, filling the activated carbon filter with activated carbon in an amount of 100 g / L according to the volume of the upper layer liquid, and the filtration speed is 5 m / h;
[0052] Step 3, adding sodium hydroxide to the upper layer liquid, the amount of sodium hydroxide added is 10 g / L, the pH value is controlled at 8, the precipitation time is 2 hours, and after the precipitation is complete, filtering is performed to obtain filtrate B;
[0053] Step 4: Add modified biochar to the filtrate B, the amount of modified biochar added is 2 g / L, the reaction time is 6 h, filter after the reaction is completed, and collect the filtered modified biochar;
[0054] The modified biochar used is surface-modified with potassium permanganate and potassium hydroxide, and the steps include: carbonizing rice husks at 600°C to obtain biochar; immersing the biochar in a 0.1 mol / L potassium permanganate solution and reacting for 1.5 hours; then taking out the biochar and immersing it in a 1 mol / L potassium hydroxide solution, reacting for 1 hour, and taking it out and drying it.
[0055] Step 5, drying the filtered modified biochar and placing it in a hydrogen reduction furnace to fill it with hydrogen, the hydrogen flow rate is controlled at 50 ml / min, the temperature of the hydrogen reduction furnace is controlled at 400°C, and the pressure is controlled at 1-10 atm. After the reaction is completed, the reduced modified biochar is taken out;
[0056] Step 6, the reduced modified biochar is ball-milled to 90 μm, then put into a reaction container, carbon monoxide is added, the temperature is controlled at 55° C. to fully react for 1 hour, and after the reaction is completed, the exhaust gas is exhausted under insulation conditions and the exhaust gas is cooled to 25° C. for condensation to obtain tetracarbonyl nickel liquid;
[0057] Step 7: thermally decompose the tetracarbon-based nickel to obtain metallic nickel.
[0058] The nickel recovery rate through the above method is 95.5%.
[0059] Example 3
[0060] A treatment process for enriching and recovering nickel from lithium battery industrial wastewater, treating 10,000L of nickel-cobalt-manganese ternary lithium battery positive electrode wastewater, the steps of which include:
[0061] Step 1: pre-filter lithium battery industrial wastewater using a grid to obtain filtrate A;
[0062] Step 2, adjusting the pH value of the A filtrate to 7.2, adding polyferric sulfate in an amount of 3 g / L according to the volume of the A filtrate, and stirring for 7 minutes, stopping stirring and waiting for the condensed particles to settle to the bottom, the sedimentation time is 3 hours, separating the upper layer liquid and passing it through an activated carbon filter, filling the activated carbon filter with activated carbon in an amount of 10 g / L according to the volume of the upper layer liquid, and the filtration speed is 8 m / h;
[0063] Step 3, adding sodium hydroxide to the upper liquid, the amount of sodium hydroxide added is 6 g / L, the pH value is controlled at 7.5, the precipitation time is 1 hour, and after the precipitation is complete, filtering is performed to obtain filtrate B;
[0064] Step 4: Add modified biochar to the filtrate B, the amount of modified biochar added is 1 g / L, the reaction time is 5 h, filter after the reaction is completed, and collect the filtered modified biochar;
[0065] The modified biochar used is surface-modified with potassium permanganate and potassium hydroxide, and the steps include: carbonizing rice husks at 550°C to obtain biochar; immersing the biochar in a 0.05 mol / L potassium permanganate solution and reacting it for 1 hour; then taking out the biochar and immersing it in a 0.5 mol / L potassium hydroxide solution and reacting it for 0.8 hours, and then taking it out and drying it.
[0066] Step 5, drying the filtered modified biochar and placing it in a hydrogen reduction furnace to fill it with hydrogen, the hydrogen flow rate is controlled at 40 ml / min, the temperature of the hydrogen reduction furnace is controlled at 300° C., and the pressure is controlled at 1-10 atm. After the reaction is completed, taking out the reduced modified biochar;
[0067] Step 6, the reduced modified biochar is ball-milled to 80 μm, then put into a reaction container, carbon monoxide is added, the temperature is controlled at 50° C. to fully react for 0.8 h, and after the reaction is completed, the exhaust gas is exhausted under insulation conditions and the exhaust gas is cooled to 22° C. for condensation to obtain tetracarbonyl nickel liquid;
[0068] Step 7: thermally decompose the tetracarbon-based nickel to obtain metallic nickel.
[0069] The nickel recovery rate through the above method is 96.1%.
[0070] The present invention also designs comparative proportions for comparison:
[0071] Comparative Example 1
[0072] A treatment process for enriching and recovering nickel from lithium battery industrial wastewater, treating 15,000L of nickel-cobalt-manganese ternary lithium battery positive electrode wastewater, the steps of which include:
[0073] Step 1: pre-filter lithium battery industrial wastewater using a grid to obtain filtrate A;
[0074] Step 2, adjusting the pH value of the A filtrate to 7, adding polyferric sulfate in an amount of 1 g / L according to the volume of the A filtrate, and stirring for 5 minutes, stopping stirring and waiting for the condensed particles to settle to the bottom, the sedimentation time is 1 hour, separating the upper layer liquid and passing it through an activated carbon filter, filling the activated carbon filter with activated carbon in an amount of 5 g / L according to the volume of the upper layer liquid, and the filtration speed is 10 m / h;
[0075] Step 3, adding sodium hydroxide to the upper layer liquid, the amount of sodium hydroxide added is 5 g / L, the pH value is controlled at 7, the precipitation time is 0.5 h, and after the precipitation is complete, filtering is performed to obtain filtrate B;
[0076] Step 4: Add biochar to the filtrate B, the amount of biochar added is 0.5 g / L, the reaction time is 3 h, filter after the reaction is completed, and collect the filtered biochar;
[0077] The biochar used comprises the following steps: carbonizing rice husks at a high temperature of 500°C to obtain the biochar.
[0078] Step 5, drying the filtered biochar and placing it in a hydrogen reduction furnace to fill it with hydrogen, with the hydrogen flow rate controlled at 30 ml / min, the temperature of the hydrogen reduction furnace controlled at 200° C., and the pressure controlled at 1-10 atm. After the reaction is completed, the reduced biochar is taken out;
[0079] Step 6, ball-mill the reduced biochar to 70 μm, then put it into a reaction container, add carbon monoxide, control the temperature at 45° C. to fully react for 0.5 h, exhaust the gas under insulation conditions after the reaction, and cool the exhaust gas to 20° C. for condensation to obtain tetracarbonyl nickel liquid;
[0080] Step 7: thermally decompose the tetracarbon-based nickel to obtain metallic nickel.
[0081] The nickel recovery rate through the above method is 60.8%.
[0082] Comparative Example 2
[0083] A treatment process for enriching and recovering nickel from lithium battery industrial wastewater, treating 15,000L of nickel-cobalt-manganese ternary lithium battery positive electrode wastewater, the steps of which include:
[0084] Step 1: pre-filter lithium battery industrial wastewater using a grid to obtain filtrate A;
[0085] Step 2, add sodium hydroxide to the A filtrate, the amount of sodium hydroxide added is 5 g / L, the pH value is controlled at 7, the precipitation time is 0.5 h, and after the precipitation is complete, filter to obtain the B filtrate;
[0086] Step 3, add modified biochar into the B filtrate, the amount of modified biochar added is 0.5 g / L, the reaction time is 3 h, filter after the reaction is completed, and collect the filtered modified biochar;
[0087] The modified biochar used is surface-modified with potassium permanganate and potassium hydroxide, and the steps include: carbonizing rice husks at 500°C to obtain biochar; immersing the biochar in a 0.01 mol / L potassium permanganate solution and reacting it for 0.5 h; then taking out the biochar and immersing it in a 0.1 mol / L potassium hydroxide solution and reacting it for 0.5 h, and then taking out and drying it.
[0088] Step 4, drying the filtered modified biochar and placing it in a hydrogen reduction furnace to fill it with hydrogen, the hydrogen flow rate is controlled at 30 ml / min, the temperature of the hydrogen reduction furnace is controlled at 200°C, and the pressure is controlled at 1-10 atm. After the reaction is completed, the reduced modified biochar is taken out;
[0089] Step 5, the reduced modified biochar is ball-milled to 70 μm, then put into a reaction container, carbon monoxide is added, the temperature is controlled at 45° C. to fully react for 0.5 h, and after the reaction is completed, the exhaust gas is exhausted under insulation conditions and the exhaust gas is cooled to 20° C. for condensation to obtain tetracarbonyl nickel liquid;
[0090] Step 6: thermally decompose the tetracarbon-based nickel to obtain metallic nickel.
[0091] The nickel recovery rate through the above method is 83.7%.
[0092] By comparing Examples 1-3 and Comparative Examples 1-2, it can be found that Examples 1-3 of the present invention maintain nickel recovery rates of more than 95%; the difference between Comparative Example 1 and the Example is that biochar is directly added without modifying the biochar, and it can be found that the nickel recovery rate is significantly reduced, and the enrichment effect is not as good as that of the Example; the difference between Comparative Example 2 and the Example is that organic matter is effectively removed, resulting in a decrease in nickel recovery rate. It is speculated that the modified biochar adsorbs organic matter and affects the enrichment effect.
[0093] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A process for enriching and recovering nickel from lithium battery industrial wastewater, characterized in that: The steps include: Step 1: pre-filter the lithium battery industrial wastewater to obtain filtrate A; Step 2, adjust the pH value of filtrate A to 7-7.5, add coagulant and stir, stop stirring and wait for the coagulated particles to settle to the bottom, separate the upper liquid and pass it through an activated carbon filter; Step 3, adding a precipitant to the upper layer liquid, controlling the pH value to be between 7 and 8, filtering after the precipitation is complete to obtain filtrate B; the precipitant is sodium hydroxide; Step 4: Add modified biochar into the filtrate B, filter after the reaction is completed, and collect the filtered modified biochar; the modified biochar used is surface-modified with potassium permanganate and potassium hydroxide; Step 5, drying the filtered modified biochar and placing it in a hydrogen reduction furnace filled with hydrogen for reduction, and taking out the reduced modified biochar after the reaction is completed; Step 6: ball-mill the reduced modified biochar, then put it into a reaction container, add carbon monoxide, control the temperature at 45-55°C for full reaction, exhaust the gas under insulation conditions after the reaction, and cool and condense the exhaust gas to obtain nickel tetracarbonyl liquid; Step 7: thermally decompose the tetracarbon-based nickel to obtain metallic nickel.
2. The process for enriching and recovering nickel from lithium battery industrial wastewater according to claim 1, characterized in that: Step 1 uses a coarse filter or a grid as a pre-filter.
3. The process for enriching and recovering nickel from lithium battery industrial wastewater according to claim 1, characterized in that: In step 2, the coagulant is polyaluminium chloride or polyferric sulfate, and the amount of coagulant added is 1-5 g / L; the stirring time is 5-10 minutes; the sedimentation time is 1-4 hours; the amount of activated carbon added to the activated carbon filter is 5-100 g / L, and the filtration speed is 5-10 m / h.
4. The process for enriching and recovering nickel from lithium battery industrial wastewater according to claim 1, characterized in that: The precipitation time in step 3 is 0.5-2h.
5. The process for enriching and recovering nickel from lithium battery industrial wastewater according to claim 1, characterized in that: In step 4, the input amount of modified biochar is 0.5-2 g / L, and the reaction time is 3-6 h.
6. The process for enriching and recovering nickel from lithium battery industrial wastewater according to claim 1, characterized in that: The preparation process of the modified biochar in step 4 includes: carbonizing the biochar source at a high temperature of 500-600°C to obtain the biochar; immersing the biochar in a potassium permanganate solution with a concentration of 0.01-0.1 mol / L and reacting for 0.5-1.5 hours; then taking out the biochar and immersing it in a potassium hydroxide solution with a concentration of 0.1-1 mol / L, reacting for 0.5-1 hour, and taking it out and drying it.
7. The process for enriching and recovering nickel from lithium battery industrial wastewater according to claim 6, characterized in that: The biochar source is selected from one or more mixtures of fruit shells, rice husks, straws and bagasse.
8. The process for enriching and recovering nickel from lithium battery industrial wastewater according to claim 1, characterized in that: In step 5, the temperature of the hydrogen reduction furnace is controlled at 200-400° C., and the pressure is controlled at 1-10 atm.
9. The process for enriching and recovering nickel from lithium battery industrial wastewater according to claim 1, characterized in that: In step 6, the modified biochar is ball-milled to 70-90 μm.
10. The process for enriching and recovering nickel from lithium battery industrial wastewater according to claim 1, characterized in that: The sufficient reaction time in step 6 is 0.5-1h; the temperature of the cooling condensation is controlled at 20-25°C.
Citation Information
Patent Citations
Modified biochar and preparation method thereof and application thereof in nickel-containing waste water
CN110152605A
Treatment method of chemical nickel plating waste liquid
CN116768424A
Method for recovering nickel metal from lithium ion battery black powder
CN116814982A
Modified cyanobacteria biachar composite material and use thereof in treatment of electroplating effluent
WO2021017455A1