Phosphorus anhydrite and preparation method thereof
Through the method of combining wet lime neutralization and low-temperature calcination, the problems of high energy consumption and waste generation in the preparation of phosphorus anhydrite are solved, and the preparation of anhydrite with high whiteness and high reactivity is achieved, which meets the requirements of green environmental protection. Require.
Patent Information
- Application Number
- CN202410738952.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-07
AI Technical Summary
The existing phosphorus anhydrite preparation technology has problems such as high energy consumption, low product whiteness and low reactivity. In addition, traditional methods will produce waste when removing harmful impurities, making it difficult to achieve green and environmental protection requirements.
The phosphogypsum is pretreated using the method of wet lime neutralization + aging, combined with low-temperature calcination at 500-550°C and the use of graphite powder to remove soluble fluorine phosphorus and organic impurities to form high whiteness anhydrous anhydrite. The generation of waste is avoided.
Obtaining high-whiteness anhydrite at low temperatures reduces production energy consumption and improves product reactivity. The process is simple, low-cost, does not produce new waste, and meets green environmental protection requirements.
Smart Images

Figure BDA0004882609650000081 
Figure BDA0004882609650000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of gypsum building materials, and in particular to phosphorus anhydrite and a preparation method thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Phosphogypsum is the main solid waste from the wet process of phosphoric acid smelting to produce phosphate fertilizers. Phosphoric acid is also the basic raw material for lithium iron phosphate. The adjustment of energy structure and the rapid development of new energy are bound to increase the demand for phosphoric acid, and the output of phosphogypsum will also grow rapidly. At present, the annual emission of phosphogypsum in the world exceeds 300 million tons, and the effective utilization rate is only about 20%. Phosphogypsum is a high-grade gypsum resource produced as a by-product of industrial phosphoric acid smelting, but harmful impurities (mainly organic matter, phosphorus, and fluorine) limit its utilization as a building material resource. At present, the main application methods of phosphogypsum are low-temperature calcination to prepare building gypsum, autoclave or normal pressure method to prepare high-strength gypsum, and high-temperature calcination to prepare anhydrous gypsum. Since harmful impurities can affect the production speed of products and reduce product performance indicators, it is necessary to take certain pretreatment measures to remove harmful impurities.
[0004] At present, the main measures to solve the adverse effects of impurities in phosphogypsum on product performance are: physical method (water washing, flotation), chemical method (acid leaching, lime neutralization), heat treatment (high temperature calcination), etc. Among them, the process of lime neutralization + high temperature calcination is relatively simple, and it can simultaneously solve the problem of deterioration of product performance caused by organic matter and soluble fluorine and phosphorus, and has received more attention. High temperature calcination of phosphogypsum to prepare anhydrous hard gypsum is considered to be a simple and feasible treatment method.
[0005] At present, the calcination temperature of the high-temperature calcination method for preparing anhydrous phosphogypsum is usually 800-1000℃. Below this temperature, the soluble fluorine and phosphorus in the phosphogypsum are difficult to convert into insoluble compounds. However, the current high-temperature calcination technology for preparing anhydrous phosphogypsum has many shortcomings, mainly including: (1) high production energy consumption; (2) low product whiteness, because when the temperature reaches about 500℃, the pyrite in the phosphogypsum will be converted into iron oxide, causing the color of the anhydrite to change from white to red, and the higher the temperature and the longer the insulation time, the darker the color; (3) the product has low reaction activity. Anhydrous gypsum can be generated at 300℃. Continuing to increase the temperature will increase the density of the anhydrite crystals, thereby reducing the reaction activity, greatly prolonging the setting time, and reducing the early strength.
[0006] Lowering the preparation temperature of anhydrous phosphate gypsum is beneficial to improving the reaction activity and whiteness of the product and saving production energy consumption, but the problem that needs to be solved to reduce the calcination temperature is how to remove the influence of harmful impurities. Washing phosphogypsum can effectively remove organic matter and soluble fluorine and phosphorus. For example, the patent with publication number CN106977123A discloses a process method for removing citric acid and water washing of impurity fluorine in phosphogypsum. The method adds citric acid water to phosphogypsum for washing, then washes the phosphogypsum sample, and finally removes impurities and dries it through a washing process. However, the scheme uses lime neutralized water to wash the phosphogypsum sample multiple times, which consumes a large amount of water and produces a large amount of sewage containing ionic impurities. While using waste, it also produces new waste, which does not meet the requirements of green environmental protection. And the method also needs to specially set up a drying process, which increases the technical complexity and preparation cost, and is difficult to implement in actual production.
[0007] Therefore, how to provide a simple method for preparing phosphorus anhydrous gypsum with high whiteness and no harmful impurities without generating waste is an urgent problem to be solved. Summary of the invention
[0008] In view of this, the present invention provides a phosphorus anhydrite and a preparation method thereof, which solves the problem that the existing preparation process of phosphorus anhydrite cannot simultaneously meet the requirements of no waste generation and high whiteness of the product and no harmful impurities.
[0009] In a first aspect, the present invention provides a method for preparing phosphorus anhydrite, comprising the following steps:
[0010] The phosphogypsum, quicklime and water are uniformly mixed and aged to obtain pretreated phosphogypsum;
[0011] The pretreated phosphogypsum and graphite powder are mixed and then heated to 500-550°C for calcination to obtain the product.
[0012] Preferably, the mass ratio of the phosphogypsum, quicklime and water is 100:(1-3):(15-20).
[0013] Preferably, the aging time is 40 to 60 hours.
[0014] Preferably, the mass ratio of the pretreated phosphogypsum to graphite powder is 100:(0.5-1).
[0015] Preferably, the calcination time is 0.5 to 3 hours.
[0016] Preferably, the calcination process is carried out under air atmosphere.
[0017] Preferably, the heating rate to 500-550° C. is 5-15° C. / min.
[0018] Preferably, the particle size of the phosphogypsum is 100-200 mesh, and the particle size of the quicklime is 100-200 mesh.
[0019] Preferably, the particle size of the graphite powder is 1 to 20 μm.
[0020] In a second aspect, the present invention provides phosphorus anhydrite prepared by the above preparation method.
[0021] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0022] (1) The preparation method of phosphorus anhydrite provided by the present invention can obtain anhydrite with high whiteness and no harmful impurities at a low calcination temperature of 500-550°C, and the whiteness can be as high as 0.7 or above, which not only greatly reduces the production energy consumption, but also effectively improves the basic activity of the product reaction;
[0023] (2) The present invention adopts the method of wet lime neutralization + aging to pretreat phosphogypsum, which can effectively remove soluble fluorine phosphorus. The removal process is simple, the energy consumption is very low, no drying treatment is required, the preparation cost is low, and no new waste is generated during the preparation process. DETAILED DESCRIPTION
[0024] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0025] The present invention provides a method for preparing phosphorus anhydrite, comprising the following steps:
[0026] The phosphogypsum, quicklime and water are uniformly mixed and aged to obtain pretreated phosphogypsum;
[0027] The pretreated phosphogypsum and graphite powder are mixed and then calcined at 500-550°C to obtain the product.
[0028] In the existing phosphogypsum pretreatment process, the reaction speed of fluorine, phosphorus and calcium in the dry lime neutralization method in the solid phase environment is slow, and a higher reaction temperature is required to accelerate the reaction (such as CN106006643A); the water washing method will produce new waste (such as CN106977123A), and the preparation of slurry lime neutralization method increases the preparation process, drying process and cost (such as CN112871457A). The present invention uses a phosphogypsum pretreatment method of wet lime neutralization + aging to adjust the pH value of phosphogypsum, accelerate the soluble phosphorus and fluorine to combine at low temperature to form insoluble matter, the insoluble matter does not participate in the hydration reaction of gypsum, and remains in the anhydrous gypsum without adversely affecting the product performance, thereby solving the adverse effects of soluble fluorine and phosphorus ions on product performance without generating waste.
[0029] The existing method of improving the whiteness of phosphogypsum products is generally to improve the whiteness of the product through a flotation process. However, the flotation process is complicated, and will produce new waste and high production cost. There is also an existing technology that adds ammonium chloride additives to phosphogypsum to whiten the calcined product of phosphogypsum. However, the content of chloride ions in gypsum is strictly controlled as harmful ions. The national standard for building gypsum requires that the chloride content is less than 0.2%. In addition, ammonium chloride will decompose and release ammonia during the calcination process, and an additional flue gas treatment device is required, which increases the production cost.
[0030] The present invention finds that the whiteness of calcined phosphogypsum is mainly affected by organic impurities and iron valence, and the organic matter in the phosphogypsum is completely decomposed at a temperature of 500°C. Therefore, the present invention improves the whiteness of anhydrite products in two ways: (1) setting the calcination temperature to 500-550°C, at which the organic impurities in the phosphogypsum can be completely removed, greatly improving the whiteness of the product; (2) adding a reducing agent, graphite, whose oxidation temperature point matches the calcination temperature, and can effectively curb the conversion of divalent iron to trivalent iron at 500-550°C, reducing the coloring effect of trivalent iron. The high-whiteness anhydrous anhydrite preparation process of the present invention is simple, the preparation cost is low, no new waste is generated, and it is conducive to actual production.
[0031] In the present invention, the mass ratio of the phosphogypsum, quicklime and water is 100:(1-3):(15-20). The present invention finds that when the quicklime dosage is too low, the soluble ions cannot be completely removed, which will have an adverse effect on the coagulation and mechanical properties of the product; if the quicklime dosage is too high, it will affect the purity of the final anhydrous hard gypsum, and there will be residues after calcination, resulting in an increase in the water demand of the anhydrous gypsum. The amount of water added in the present invention satisfies the accumulation pores in the powder to produce a micro-liquid phase environment, which is conducive to the soluble fluorine and phosphorus ions and calcium ions to combine to form insoluble precipitates. If the amount of water added is too little, a liquid phase cannot be formed, and the lime cannot be dissolved to produce soluble calcium ions and combine with soluble fluorine and phosphorus ions. If too much water is added, a slurry is formed, which needs to be dried after aging, and agglomerates after drying. Secondary grinding is required before calcination, and the process is highly complex and the production cost increases.
[0032] The present invention does not impose any special restrictions on the aging process, and the aging operation known in the art can be used. In the present invention, the aging time is 40 to 60 hours, more preferably 45 to 50 hours, and most preferably 48 hours.
[0033] In the present invention, the mass ratio of the pretreated phosphogypsum to the graphite powder is 100:(0.5-1). When the amount of graphite powder added is insufficient, the conversion of iron sulfide to iron oxide cannot be effectively inhibited, and the whiteness of the product decreases; too high an amount will have an adverse effect on the whiteness of the phosphogypsum anhydrite product.
[0034] In the present invention, the calcination time is 0.5 to 3 hours, more preferably 1 to 2 hours. During the calcination process, the phosphogypsum is gradually dehydrated to form anhydrous phosphogypsum, and the impurities and organic matter are completely decomposed.
[0035] In the present invention, the calcination process is carried out in an air atmosphere. The heating rate to 500-550° C. is 5-15° C. / min, more preferably 8-12° C. / min.
[0036] In the present invention, in order to allow soluble fluoride and phosphorus ions to fully react with calcium ions to generate insoluble precipitates, the particle size of the phosphogypsum of the present invention is 100-200 meshes, more preferably 150 meshes; the particle size of the quicklime is 100-200 meshes, more preferably 150 meshes.
[0037] In the present invention, the particle size of the graphite powder is 1 to 20 μm, more preferably 5 to 15 μm.
[0038] The present invention also provides phosphorus anhydrite prepared by the above preparation method. The phosphorus anhydrite prepared by the present invention does not contain organic matter and soluble phosphorus and fluorine impurities, and has a high whiteness, which can reach above 0.7.
[0039] The technical solution of the present invention is further described below in conjunction with specific embodiments. In the following embodiments, the particle size of quicklime powder is 150 mesh, and the average particle size of graphite powder is 10 μm.
[0040] Example 1
[0041] This embodiment provides a method for preparing phosphorus anhydrous gypsum.
[0042] (1) Wet pretreatment: grind the phosphogypsum powder through a 150-mesh sieve, weigh 100 g of phosphogypsum, 15 g of water and 2 g of quicklime powder, stir evenly and age for 48 h to obtain pretreated phosphogypsum;
[0043] (2) Calcination process: 100 g of pretreated phosphogypsum and 0.8 g of graphite powder were mixed and placed in a high-temperature furnace. The temperature was raised to 550 °C at a rate of 10 °C / min. After being kept at this temperature for 2 h, the mixture was cooled to room temperature in the furnace and then taken out to obtain anhydrous phosphogypsum.
[0044] Example 2
[0045] This embodiment provides a method for preparing phosphorus anhydrous gypsum.
[0046] (1) Wet pretreatment: grind the phosphogypsum powder through a 150-mesh sieve, weigh 100 g of phosphogypsum, 18 g of water and 2.5 g of quicklime powder, stir evenly and age for 48 h to obtain pretreated phosphogypsum;
[0047] (2) Calcination process: 100 g of pretreated phosphogypsum and 0.8 g of graphite powder were mixed and placed in a high-temperature furnace. The temperature was raised to 510 °C at a rate of 10 °C / min. After being kept at this temperature for 2 h, the mixture was cooled to room temperature in the furnace and then taken out to obtain anhydrous phosphogypsum.
[0048] Example 3
[0049] This embodiment provides a method for preparing phosphorus anhydrous gypsum.
[0050] (1) Wet pretreatment: grind the phosphogypsum powder through a 150-mesh sieve, weigh 100 g of phosphogypsum, 15 g of water and 1.5 g of quicklime powder, stir evenly and age for 48 h to obtain pretreated phosphogypsum;
[0051] (2) Calcination process: 100 g of pretreated phosphogypsum and 1 g of graphite powder were mixed and placed in a high-temperature furnace. The temperature was raised to 550 °C at a rate of 10 °C / min. After being kept at this temperature for 2 h, the mixture was cooled to room temperature in the furnace and then taken out to obtain anhydrous phosphogypsum.
[0052] Example 4
[0053] This embodiment provides a method for preparing phosphorus anhydrous gypsum.
[0054] (1) Wet pretreatment: grind the phosphogypsum powder through a 150-mesh sieve, weigh 100 g of phosphogypsum, 15 g of water and 2 g of quicklime powder, stir evenly and age for 45 h to obtain pretreated phosphogypsum;
[0055] (2) Calcination process: 100 g of pretreated phosphogypsum and 0.5 g of graphite powder were mixed and placed in a high-temperature furnace. The temperature was raised to 525 °C at a rate of 8 °C / min. After being kept at this temperature for 2 h, the mixture was cooled to room temperature in the furnace and then taken out to obtain anhydrous phosphogypsum.
[0056] Comparative Example 1
[0057] Compared with Example 1, the difference between this comparative example is that the amount of quicklime powder is 0.5g.
[0058] Comparative Example 2
[0059] Compared with Example 1, the difference between this comparative example and Example 1 is that the pretreatment is dry-mixed lime neutralization, and the specific operation steps are as follows:
[0060] Grind the phosphogypsum powder through a 150-mesh sieve, weigh 100 g of phosphogypsum and 2 g of quicklime powder, stir evenly and age for 48 hours to obtain pretreated phosphogypsum; mix 100 g of pretreated phosphogypsum with 0.8 g of graphite powder, place in a high-temperature furnace, heat to 550°C at a rate of 10°C / min, keep warm for 2 hours, cool to room temperature with the furnace, and take out.
[0061] Comparative Example 3
[0062] The difference between this comparative example and Example 1 is that no graphite powder is added in this comparative example.
[0063] Comparative Example 4
[0064] The difference between this comparative example and Example 1 is that the temperature is increased to 450° C. at a rate of 10° C. / min.
[0065] Comparative Example 5
[0066] Compared with Example 1, this comparative example is different in that: this comparative example does not perform wet pretreatment. The specific steps are as follows:
[0067] Grind the phosphogypsum powder through a 150-mesh sieve, mix 100g of phosphogypsum with 0.8g of graphite powder, place in a high-temperature furnace, heat to 550℃ at a rate of 10℃ / min, keep warm for 2h, cool to room temperature with the furnace, and take out.
[0068] Comparative Example 6
[0069] Compared with Example 1, the difference between this comparative example and Example 1 is that: this comparative example does not perform wet pretreatment, does not add graphite powder, and calcines phosphogypsum at 550°C. The specific steps are as follows:
[0070] Grind the phosphogypsum powder through a 150-mesh sieve, then place it in a high-temperature furnace, heat it to 550°C at a rate of 10°C / min, keep it warm for 2 hours, cool it to room temperature with the furnace, and take it out.
[0071] Comparative Example 7
[0072] Compared with Example 1, the difference between this comparative example and Example 1 is that: this comparative example does not perform wet pretreatment, does not add graphite powder, and calcines phosphogypsum at 850°C. The specific steps are as follows:
[0073] Grind the phosphogypsum powder through a 150-mesh sieve, then place it in a high-temperature furnace, heat it to 850°C at a rate of 10°C / min, keep it warm for 2 hours, cool it to room temperature with the furnace, and take it out.
[0074] The performance of the final products of Example 1 and Comparative Examples 1 to 7 was measured, as shown in Table 1. Note: The mechanical property data (3d compressive strength, 28d compressive strength) in Table 1 are experimental values when no active activator is added.
[0075] Table 1 Final product performance measurement data of Example 1 and Comparative Examples 1 to 7
[0076]
[0077]
[0078] It can be seen from Table 1 that the phosphorus anhydrite of Example 1 has the highest whiteness value, which can reach 75%, and has excellent mechanical properties and a high degree of hydration.
[0079] In Comparative Example 1, the amount of quicklime added is relatively low. In the wet mixing pretreatment stage, the soluble fluorine and phosphorus ions cannot be completely combined to form insoluble substances, which has an adverse effect on the coagulation performance and mechanical properties of the product.
[0080] In Comparative Example 2, a dry lime pretreatment process was used. In the absence of a liquid phase, the chemical reaction rate between Ca ions and soluble fluoride and phosphorus ions was extremely low, resulting in a high soluble fluoride and phosphorus content in the product, which was detrimental to the coagulation and mechanical properties.
[0081] In Comparative Example 3, graphite powder is not added, and the whiteness is greatly reduced compared with Example 1. This is because when there is no reducing agent, the divalent iron sulfide in the phosphogypsum is oxidized to red trivalent iron at about 500°C, reducing the whiteness of the product. The calcination temperature of Comparative Example 4 is reduced to 450°C, and it can be seen that the whiteness of the product is significantly reduced. This is because the temperature is low and the organic matter cannot be completely decomposed and removed, which reduces the whiteness of the product; the mechanical properties of the obtained product are reduced, mainly because the residual organic matter has an adverse effect on the mechanical properties, and the amount of type II anhydrous gypsum generated in the product is lower at a lower temperature.
[0082] Comparative Example 5 does not undergo wet pretreatment, and it can be seen that the coagulation performance and mechanical properties of the product are both low, because the product contains soluble phosphorus and fluorine impurities, which have an adverse effect on the coagulation performance and mechanical properties of the product. The whiteness of the product of Comparative Example 5 is higher than that of Comparative Example 6, because the graphite powder in Comparative Example 5 can inhibit the coloring effect of trivalent iron.
[0083] Comparative Example 7: Phosphogypsum is calcined at 850°C. Since the pyrite in the phosphogypsum is converted into iron oxide, the color of the anhydrite changes from white to red, so its whiteness is very low, only 52%. At the same time, the high temperature treatment at 850°C will increase the density of the anhydrite crystals, thereby reducing the reaction activity, greatly prolonging the setting time, and reducing the compressive strength.
[0084] The impurity content of the final products of Example 1, Comparative Example 4, Comparative Example 6 and Comparative Example 7 was measured, as shown in Table 2.
[0085] Table 2 Impurity content of phosphorus anhydrous gypsum products (%)
[0086] Example / Comparative Example Organic matter Soluble Phosphorus Soluble fluoride Example 1 0 0 0 Comparative Example 4 0.12 0 0 Comparative Example 6 0 1.3 0.77 Comparative Example 7 0 0 0
[0087] As can be seen from Table 2, after wet pretreatment but when the calcination temperature is low (Comparative Example 4), it is difficult to completely remove organic matter. Combined with Table 1, it can be seen that the presence of organic matter will have an adverse effect on the whiteness and mechanical properties of the product. Without wet pretreatment and without adding graphite powder, only calcining the phosphogypsum at 550°C (Comparative Example 6), soluble phosphorus and fluorine will exist in the product. Calcination at 850°C can completely remove soluble phosphorus and fluorine and organic matter, which is also a common impurity removal method for phosphorus anhydrous hard gypsum in the prior art. Example 1 of the present invention can remove organic matter and soluble phosphorus and fluorine at a lower temperature through wet pretreatment + calcination at 550°C.
[0088] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing phosphorus anhydrite, It is characterized in that The steps include: The phosphogypsum, quicklime and water are uniformly mixed and aged to obtain pretreated phosphogypsum; The pretreated phosphogypsum and graphite powder are mixed and then heated to 500-550°C for calcination to obtain the product.
2. The preparation method according to claim 1, It is characterized in that The mass ratio of the phosphogypsum, quicklime and water is 100:(1-3):(15-20).
3. The preparation method according to claim 1, It is characterized in that The aging time is 40 to 60 hours.
4. The preparation method according to claim 1, It is characterized in that The mass ratio of the pretreated phosphogypsum to the graphite powder is 100:(0.5-1).
5. The preparation method according to claim 1, It is characterized in that The calcination time is 0.5 to 3 hours.
6. The preparation method according to claim 1, It is characterized in that The calcination process is carried out under air atmosphere.
7. The preparation method according to claim 1, It is characterized in that The heating rate to 500-550°C is 5-15°C / min.
8. The preparation method according to claim 1, It is characterized in that The particle size of the phosphogypsum is 100-200 meshes, and the particle size of the quicklime is 100-200 meshes.
9. The preparation method according to claim 1, It is characterized in that The particle size of the graphite powder is 1 to 20 μm.
10. Phosphorus anhydrite prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for producing building powdered gypsum by using phosphogypsum
CN102390942A
Preparation process of desulfurized gypsum
CN107804985A
Treatment process of industrial waste phosphogypsum
CN111138102A
Production process of multifunctional paper-faced gypsum board
CN111421653A
Gypsum powder production system and process
CN112876110A