Castable for baking-free coke pot lining or working layer, application of castable and coke pot

By using non-bake castables and polymer insulation boards made of mullite and other materials, the problem of easy oxidation and deformation of dry quenching coke tank linings at high temperatures has been solved, and the service life of the coke tank has been extended and production has been achieved. The cost reduction reduces environmental pollution and maintenance workload.

CN118724573APending Publication Date: 2024-10-01BAOSHAN IRON & STEEL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310335355.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing dry quenching coke tank linings are prone to oxidation, deformation, and cracking at high temperatures, resulting in reduced strength and short service life of the coke tank. In addition, the cost of lining spare parts is high, the maintenance workload is heavy, and there are potential safety hazards and environmental pollution problems.

Method used

The no-bake castable made of mullite, corundum, nano-alumina, spodumene, sintering agent, binding agent and steel fiber is used as the lining of the coke tank, combined with low thermal conductivity polymer insulation board and anchor nails. The tank structure is formed to improve heat resistance and service life.

Benefits of technology

The castable can be used without high-temperature baking, which improves the overall performance and operational stability of the coke tank, extends its service life, reduces production costs and environmental pollution, and reduces maintenance time and worker labor intensity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a castable for a baking-free coke pot lining or a working layer, application and a coke pot. The castable is a mixture of the following components in percentage by mass: 60%-79% of mullite, 8%-12% of corundum, 3%-5% of silicon powder, 3%-5% of nano aluminum oxide, 3%-6% of spodumene, 1%-4% of a sintering agent, 1%-3% of a binding agent and 2%-5% of SiOxX-Zero. 0.2%-0.5% of explosion-proof fibers and 1%-3% of steel fibers are additionally arranged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a casting material, in particular to a casting material for the inner lining or working layer of a non-baking coke tank, its application and the coke tank. Background Art

[0002] The CDQ coke tank plays a key role in quenching and storing coke in CDQ production. The safety and stability of the overall quality of the coke tank is directly related to the continuous and effective operation of the entire CDQ production system. The safety and stability of the equipment is the greatest guarantee for the production and operation of the CDQ system, and also the greatest cost reduction. Currently, the CDQ coke tank structure is generally a steel frame with an alloy liner inlaid structure. During the production and operation process, there are mainly the following problems:

[0003] (1) When the coke is taken out of the furnace, the temperature reaches over 1000℃. The lining plate and steel frame structure of the coke drum are prone to oxidation, deformation and cracking due to the high temperature, which causes the strength of the outer frame of the tank to decrease, break and deform, and the lining plate is prone to carbonization, wear and fall off. In this case, the rotary sealing valve motor is prone to burnout, causing safety accidents such as bumps, scalds and even poisoning to the maintenance personnel. The safety hazard is relatively large, seriously affecting the overall service life of the tank body and bringing great risks to the enterprise.

[0004] (2) Due to the large consumption of linings, the cost of spare parts for linings is high, and the workload of workers for maintenance is heavy, resulting in excessive economic burden and affecting the overall profit of the enterprise.

[0005] (III) The coke tank is made of all-steel structure, and the thermal conductivity of steel is high. When the coke tank is in operation, the shell temperature is as high as 600℃ or more, resulting in large heat loss and burning. At the same time, during the transportation of red coke, it is inevitable to produce convection heat exchange and radiation heat exchange with the air. A large amount of air enters the coke tank through the gaps in the lining plate and burns in contact with the red coke, increasing the burning loss of coke. Due to the high ambient temperature, it is not conducive to meeting environmental protection standards.

[0006] Therefore, the various performances of the coke drum lining currently directly affect the service life of the coke drum. How to increase the service life of the coke drum and improve the performance of the coke drum working layer is the most critical. Therefore, improving the performance of the coke drum lining material has become the key to extending the service life of the coke drum. Summary of the invention

[0007] In view of the above-mentioned technical problems of the existing coke drum, the technical problem to be solved by the present invention is to replace the existing ductile iron or cast steel lining, provide a special castable for coke drum that is in direct contact with the red coke, and can eliminate the need for refractory materials to be baked at high temperature before use, thereby improving the comprehensive performance and operating stability of the coke drum and greatly increasing the service life of the coke drum.

[0008] The technical problem to be solved can be implemented through the following technical solutions.

[0009] A castable for the lining or working layer of a non-bake coke tank, characterized in that the castable is a mixture of the following components in mass percentage:

[0010] Mullite 60% to 79%, corundum 8% to 12%, silicon powder 3% to 5%, nano-alumina 3% to 5%, spodumene 3% to 6%, sintering agent 1% to 4%, binder 1% to 3%, SiOxX-Zero 2% to 5%; and

[0011] The added explosion-proof fiber is 0.2% to 0.5% and the steel fiber is 1% to 3%.

[0012] Preferably, the particle size of the mullite is ≤10 mm.

[0013] Preferably, the sintering agent is Yixing white mud.

[0014] Preferably, the critical particle size of the castable is 5 to 10 mm.

[0015] Preferably, the steel fiber is made of 304 material.

[0016] Another technical problem to be solved by the present invention is to provide an application of the aforementioned castable as a lining material or a working layer material of a dry coke quenching drum.

[0017] Another technical problem to be solved by the present invention is to provide a coke tank, whose tank structure comprises, from outside to inside, a tank inner wall layer, an insulation board layer and a castable casting layer; the castable casting layer is cast by mixing the above-mentioned castables.

[0018] Furthermore, anchor nails which are welded and fixed on the inner wall of the tank body are pre-embedded in the casting layer of the casting material, and the surface of the anchor nails is coated with an asphalt layer.

[0019] Furthermore, the thermal insulation board layer is a polymer-bonded nano thermal insulation board with low thermal conductivity.

[0020] Furthermore, the asphalt layer is formed by applying asphalt paint several times.

[0021] When the castable adopts the above technical scheme and is used for the lining or working layer of the coke tank, the process of high-temperature baking of the refractory material can be eliminated, which can save maintenance time, production cost, improve economic benefits and reduce environmental pollution for the enterprise. The castable adopts mullite with high strength, good wear resistance, strong thermal shock stability and low thermal conductivity as aggregate and corundum as matrix material. The addition of spodumene, nano-powder and sintering agent improves the density, thermal shock resistance and strength of the material. At the same time, the addition of special additives allows the castable to be used after pouring as long as it is naturally cured for 5 to 7 days without rain. In addition, the preparation and implementation method of the special castable for the coke tank without baking of the present invention is not only simple and easy to operate, but also has moderate product body density; easy to construct, high temperature strength, excellent wear resistance; low thermal conductivity, good thermal shock resistance, and can ensure the long-term stable, reliable and safe operation of the coke tank lining quality. It can greatly improve the service life of the overall coke tank and the service life of the lining, which is more than 50% higher than the original lining life. DETAILED DESCRIPTION

[0022] The specific embodiments of the present invention are described in further detail below.

[0023] The coke drum of the existing coking system is generally a columnar frame structure with a ductile iron or cast steel lining. It has a high operating temperature and the outer shell temperature reaches over 600°C during operation. Due to sudden changes in temperature during operation, the columnar frame structure of the coke drum is prone to deformation and cracking due to high temperature, and has a short service life. The lining is also easily oxidized, deformed, cracked and fallen off due to high temperature and corrosive gases, posing a serious hidden danger to production continuity and production safety. Therefore, in order to cope with the above-mentioned shortcomings, the present invention has carried out a technical structural transformation on the existing coke tank, and replaced the original ductile iron or cast steel lining with an amorphous mullite castable lining. After actual use, this new structure can play a better role in over-temperature management and extend the service life of the coke tank. The surface temperature of the coke tank can be reduced to below 200°C, and because the refractory material has high bonding strength, good wear resistance, and excellent hot and cold rapid change performance, at the same time, after the lining refractory material is poured, it can be used as long as it is naturally cured for 5 to 7 days without rain, eliminating the link that the original refractory material must be baked at high temperature before it can be used, saving maintenance time for the enterprise, saving production costs, improving economic benefits, and reducing environmental pollution. It can fully meet the requirements of long-term stable operation of the coke tank, and the biggest advantage of this refractory structure is that it can be maintenance-free during the use period, saving a lot of manpower and material resources for the enterprise, reducing the labor intensity of workers, reducing environmental pollution, and increasing the economic benefits of the enterprise.

[0024] When the baking-free refractory material of the coke drum is used as the lining, the special castable, anchor nails and polymer bonded insulation board of the baking-free coke drum are utilized, and a combination mode is adopted. The optimal anchor assembly anti-thermal stress shape structure is determined through module testing and temperature detection, thus realizing the innovation of the lining structure.

[0025] The implementation process includes the following steps:

[0026] 1) Ingredients: Mullite is used as the main raw material, corundum is used as the matrix material, and nano-alumina, spodumene, sintering agent, binder, silicon powder, special additives (SiOxx Zero) and additional explosion-proof fiber and steel fiber are added.

[0027] 2) Mixing: First, add the weighed mullite aggregate and fine material into the mixer according to the corresponding proportion, and then add the weighed corundum fine powder and silicon powder, spodumene, nano alumina, sintering agent, special additives and additional explosion-proof fiber and steel fiber and stir for 3 to 5 minutes to make it uniform.

[0028] 3) Packaging: First weigh the mixture and bag it according to the requirements, then weigh and pack the binder in a small plastic bag, put it into the bag of the mixture, and seal it together. The packaging bag is a paper bag with a composite waterproof film inside and outside, and the packaging weight of each bag is 40kg.

[0029] 4) Lining pouring

[0030] Butterfly-shaped anchor nails of 200x160mm are welded inside the coke drum; the height of the butterfly-shaped anchor nails is 60-80mm depending on the location. The welding must be firm and acceptance must be carried out by hammering.

[0031] A low-thermal-conductivity polymer-bonded nano-insulation board is pasted 10mm on the inner surface of the coke tank (anchor nails need to be avoided); after the anchor nails are firmly welded, they are painted twice with asphalt paint, and then the baking-free castable is cast. After forming, the anchor nails protruding from the surface of the coke tank are buried inside the casting layer to fix the casting layer. By adding a layer of insulation (i.e., polymer-bonded insulation board) between the coke tank body and the castable, the temperature of the coke tank shell can be effectively reduced.

[0032] The following are more specific embodiments of the casting material of the present invention.

[0033] Embodiment 1:

[0034] A casting material, wherein the weight percentage of each component is:

[0035] Mullite is 70%, corundum is 8%, silicon powder is 3%, nano-alumina is 5%, sintering agent is 4%, binder is 1%, spodumene + special additives are 9%; and additional explosion-proof fiber is 0.5%, steel fiber is 1%, and water is 6.2%.

[0036] The test index of the above ratio experiment is: specific gravity after burning at 1100℃ is 2.45g / cm 3 ; Flexural resistance 12Mpa; Compression resistance 102Mpa; Abrasion resistance 7.16cm 3; Thermal shock stability>35 times; Re-firing line change -0.12%; The test strip can be directly fired in an electric furnace above 650℃ after natural curing for 5 to 7 days in an environment without rain, without bursting or cracking.

[0037] Embodiment 2:

[0038] A casting material, wherein the weight percentage of each component is:

[0039] Mullite is 68%, corundum is 9%, silicon powder is 4%, nano-alumina is 5%, sintering agent is 4%, binder is 2%, spodumene + special additives is 8%; and additional explosion-proof fiber is 0.5%, steel fiber is 2%, and water is 6.3%.

[0040] The test index of the above ratio experiment is: specific gravity after burning at 1100℃ is 2.47g / cm 3 ; Flexural resistance 11Mpa; Compression resistance 100Mpa; Abrasion resistance 7.26cm 3 ; Thermal shock stability>35 times; Re-firing line change -0.12%; The test strip can be directly added to the electric furnace above 670℃ for firing after natural curing for 5 to 7 days in an environment without rain, without bursting or cracking.

[0041] Embodiment three:

[0042] A casting material, wherein the weight percentage of each component is:

[0043] Mullite is 72%, corundum is 7%, silicon powder is 3%, nano-alumina is 4%, sintering agent is 2%, binder is 2%, spodumene + special additives is 10%; and additional explosion-proof fiber is 0.5%, steel fiber is 2%, and water is 6.5%.

[0044] The test index of the above ratio experiment is: specific gravity after burning at 1100℃ is 2.41g / cm 3 ; Flexural resistance 11Mpa; Compression resistance 105Mpa; Abrasion resistance 7.4cm 3 ; Thermal shock stability>35 times; Re-firing line change -0.13%; The test strip can be directly added to the electric furnace above 670℃ for firing after natural curing for 5 to 7 days in an environment without rain, without bursting or cracking.

Claims

1. A castable material for the lining or working layer of a non-baking coke tank, characterized in that: The castable is a mixture of the following components in percentage by mass: Mullite 60% to 79%, corundum 8% to 12%, silicon powder 3% to 5%, nano-alumina 3% to 5%, spodumene 3% to 6%, sintering agent 1% to 4%, binder 1% to 3%, SiOxX-Zero 2% to 5%; and The added explosion-proof fiber is 0.2% to 0.5% and the steel fiber is 1% to 3%.

2. The castable material for the lining or working layer of the unbaked coke tank according to claim 1, characterized in that: The particle size of the mullite is ≤10 mm.

3. The castable material for the lining or working layer of the unbaked coke tank according to claim 1, characterized in that: The sintering agent is Yixing white mud.

4. The castable material for the lining or working layer of the unbaked coke tank according to claim 1, characterized in that: The critical particle size of the castable is 5 to 10 mm.

5. The castable material for the lining or working layer of the unbaked coke tank according to claim 1, characterized in that: The steel fiber is made of 304 material.

6. Use of the castable according to any one of claims 1 to 5 as a lining material or working layer material for a dry coke quenching drum.

7. A coke tank, characterized in that: The tank structure comprises, from outside to inside, a tank inner wall layer, an insulation board layer and a castable casting layer; the castable casting layer is formed by mixing and casting the castable described in any one of claims 1 to 5.

8. The coke tank according to claim 7, characterized in that: Anchor nails are pre-buried in the casting layer of the casting material and are welded and fixed on the inner wall of the tank body. The surface of the anchor nails is coated with an asphalt layer.

9. The coke tank according to claim 7, characterized in that: The thermal insulation board layer is a low thermal conductivity polymer combined nano thermal insulation board.

10. The coke tank according to claim 8, characterized in that: The asphalt layer is formed by applying asphalt paint several times.

Citation Information

Patent Citations

  • Pouring material for producing high-temperature ceramic abrasion-proof lining body

    CN101172847A

  • A rapid repairing material for bracket parts of inclined flues of coke dry quenching furnaces and a repairing method thereof

    CN106242599A

  • Wear-resistant castable and preparation and application method thereof

    CN109020585A

  • Cordierite-containing composite refractory material for working linings of coke dry quenching tank and bin body

    CN111978077A

  • Quick baking castable containing SioxX Zero and application of quick baking castable in aluminum industry

    CN113511903A