Photocatalytic synthesis method and application of Spiro-OMeTAD

Through the photocatalytic synthesis method, the problems of low conversion rate in the preparation of spiro-OMeTAD and the impact of Li-TFSI oxidation on the stability of perovskite solar cells were solved, and the preparation of Spiro-OMeTAD with high conductivity and high purity was achieved, improving the performance of solar cells. Performance and stability.

CN118724730APending Publication Date: 2024-10-01WUHAN HISPRING TECH DEV CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410726012.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the prior art, the preparation conversion rate of spiro-OMeTAD is low and Li-TFSI doping oxidation affects the stability of perovskite solar cells.

Method used

Using a photocatalytic synthesis method, 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 4,4'-dimethoxydiphenylamine, alkali metal alkoxide, photosensitive catalyst and The ligand is dissolved in an organic solvent, and light with a wavelength of 400 to 780 nm is applied to obtain highly conductive and high-purity Spiro-OMeTAD, which simultaneously oxidizes the molecules to avoid hygroscopicity and ion migration of the lithium salt.

Benefits of technology

Significantly improves the chemical substitution selectivity of Spiro-OMeTAD, reduces the generation of isomer impurities, obtains high conductivity and high purity products, avoids the impact of lithium salts on the performance of optoelectronic devices, shortens the preparation cycle and reduces costs .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724730A_ABST
    Figure CN118724730A_ABST
Patent Text Reader

Abstract

The invention discloses a photocatalytic synthesis method and application of Spiro-OMeTAD, and the synthesis method comprises the following steps: dissolving 2, 2 ', 7, 7'-tetrabromo-9, 9 '-spirobifluorene, 4, 4'-dimethoxydiphenylamine, alkali metal alkoxide, a photosensitive catalyst and a ligand in an organic solvent, and uniformly stirring; illumination is applied to the solution system in the step a) for 1-48 h, and Spiro-OMeTAD is obtained through aftertreatment; the wavelength of the illumination ranges from 400 nm to 780 nm, and the intensity of the illumination ranges from 1000 Lux to 30000 Lux. According to the photocatalytic synthesis method, the purity and the yield of the product can be improved, Spiro-OMeTAD molecules can be synchronously oxidized in the photocatalytic reaction process to form Spiro-OMeTAD oxidation-state molecules which are free of lithium salt doping and high in conductivity, the influence of lithium salt moisture absorption and ion migration on the performance of corresponding photoelectric devices can be effectively avoided, and the application process of the Spiro-OMeTAD molecules is accelerated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hole transport materials, in particular to a photocatalytic synthesis method and application of Spiro-OMeTAD. Background Art

[0002] Metal halide perovskites are cheap and easy to process in solutions. Within a decade, perovskite solar cells have achieved a power conversion efficiency of up to 26%, which is almost comparable to the highest efficiency of silicon cells. In perovskite solar cells, the organic semiconductor film sandwiched between the absorption layer and the electrode is an important component for achieving high-efficiency devices. The use of dopants in the hole transport layer can improve the mobility of the hole transport layer (HTL) and optimize the energy level matching between the hole transport layer and the perovskite, which is crucial to achieving a high conversion efficiency (PCE) of formal perovskite solar cells.

[0003] 2,2',7,7'-Tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (spiro-OMeTAD, CAS: 207739-72-8) has excellent charge transport ability due to the presence of a conjugated molecular skeleton. It can effectively collect and transport holes, thereby improving the photoelectric conversion efficiency of solar cells. Therefore, it is often used as a hole transport material.

[0004] However, the preparation of spiro-OMeTAD in the prior art is usually prepared by palladium catalysis using halogenated spirobifluorene and 4,4'-dimethoxydiphenylamine, and the reaction conversion rate of this process is low. In addition, Chinese patent document CN1582270A discloses that the CN-coupling reaction process is easily occupied by other atoms next to the halogen atom to produce isomers.

[0005] The conductivity of pure spiro-OMeTAD is very low, and doping can change the electronic properties of organic semiconductors. The conventional doping method is to use lithium bis(trifluoromethylsulfonyl)imide (Li-TFSI) as a dopant in the hole transport layer Spiro-OMeTAD, and then expose the spiro-OMeTAD:LiTFSI film to air and light for post-treatment. In this oxidation process, due to the auxiliary effect of LiTFSI, spiro-OMeTAD is irradiated by ultraviolet light and oxidized by oxygen in the ambient air, and the oxidation product acts as a dopant to achieve hole transport. Lithium oxide also remains in the film as a by-product. In addition, Li-TFSI is not only hygroscopic, but lithium ions will spontaneously migrate to adjacent functional layers, especially perovskite. This is one of the main factors affecting the long-term stability of perovskite solar cells.

[0006] Therefore, it is necessary to propose a new spiro-OMeTAD preparation process to solve the problems of low conversion rate in the existing technology and the subsequent Li-TFSI doping oxidation affecting the stability of perovskite solar cells. Summary of the invention

[0007] The present invention provides a photocatalytic synthesis method and application of Spiro-OMeTAD, which are used to solve the problems of low conversion rate of Spiro-OMeTAD prepared in the prior art and influence of subsequent Li-TFSI doping oxidation on the stability of perovskite solar cells.

[0008] In view of this, the scheme of the present invention is:

[0009] The first aspect of the present invention provides a photocatalytic synthesis method of Spiro-OMeTAD, comprising the steps of:

[0010] a) dissolving 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 4,4'-dimethoxydiphenylamine, alkali metal alkoxide, photosensitive catalyst and ligand in an organic solvent and stirring uniformly;

[0011] b) applying light to the solution system of step a) for 1 to 48 hours, and then performing post-treatment to obtain Spiro-OMeTAD; the light wavelength is 400 to 780 nm, and the intensity is 1000 to 30000 Lux.

[0012] Furthermore, the illumination conditions are: wavelength 400nm, intensity 30000Lux, and illumination duration 1h.

[0013] Furthermore, the molar ratio of the 4,4'-dimethoxydiphenylamine to the 2,2',7,7'-tetrabromo-9,9'-spirobifluorene is (1-4):1.

[0014] Furthermore, the photosensitive catalyst is selected from titanium dioxide, Ru(bpy)3Cl2, Co(bpy)3C l2 , Fe(bpy)3Cl2, single-atom palladium, PhCH(CN)2, Ir(ppy)2(dtbbpy)(PF6), preferably Co(bpy)3C l2 ; and / or, the molar amount of the photosensitive catalyst is 0.01-0.1% of the total molar amount of the reaction substrate.

[0015] Furthermore, the ligand is selected from one of 1,1'-binaphthyl-2,2'-bisdiphenylphosphine, 4,5-bisdiphenylphosphine-9,9-dimethylxanthene, 1,1'-bis(diphenylphosphino)ferrocene, tri-tert-butylphosphine, and tri-tert-butylphosphine tetrafluoroborate.

[0016] Furthermore, the organic solvent is selected from commonly used organic solvents such as tetrahydrofuran or toluene.

[0017] Furthermore, step a) is carried out under an inert atmosphere.

[0018] The second aspect of the present invention provides Spiro-OMeTAD obtained by the photocatalytic synthesis method described in the first aspect.

[0019] Furthermore, the electrical conductivity of the Spiro-OMeTAD is greater than 1.0×10 -4 S / cm.

[0020] According to a third aspect of the present invention, a solar cell is provided, comprising a hole transport layer and a perovskite layer; the hole transport layer comprises the Spiro-OMeTAD described in the second aspect.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The photocatalytic preparation method provided by the present invention obtains Spiro-OMeTAD with high conductivity, high purity and high yield. Through the specific active sites of the photosensitive catalyst, the process of generating Spiro-OMeTAD has better chemical substitution selectivity, reducing the generation of impurities of Spiro-OMeTAD isomer derivatives; in addition, the Spiro-OMeTAD molecules can be simultaneously oxidized during the photocatalytic reaction to form Spiro-OMeTAD oxidized state molecules without lithium salt doping and high conductivity, which can effectively avoid the influence of lithium salt moisture absorption and ion migration on the performance of corresponding photoelectric devices. The invention can significantly shorten the preparation cycle of oxidized Spiro-OMeTAD, reduce the preparation cost, and accelerate the application process of Spiro-OMeTAD molecules. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Schematic diagram of the structure of Spiro-OMeTAD and its isomers described in the present invention.

[0024] Figure 2 This is a schematic diagram of the overall reaction process of the photocatalytic preparation of Spiro-OMeTAD in the present invention. DETAILED DESCRIPTION

[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the preferred embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] like Figure 1As shown in the figure, multiple isomers are usually produced during the preparation of Spiro-OMeTAD. The slight differences in the molecular structure of the isomers affect the electronic properties and intermolecular interactions, thereby affecting the energy level matching and molecular stacking, and further affecting the hole mobility of the material. In addition, low-purity spiro-OMeTAD contains more impurities and defects, which will reduce the effective mobility of holes. The improvement of hole transport performance directly affects the fill factor (FF) and photoelectric conversion efficiency (PCE) of solar cells. High-purity Spiro-OMeTAD with an optimized isomer ratio can significantly improve the above performance parameters of the device.

[0027] In one embodiment, Figure 2 As shown, a photocatalytic synthesis method of Spiro-OMeTAD is proposed, and the steps include:

[0028] a) dissolving 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 4,4'-dimethoxydiphenylamine, alkali metal alkoxide, photosensitive catalyst and ligand in an organic solvent and stirring uniformly;

[0029] b) applying light to the solution system of step a) for 1 to 48 hours, and then performing post-treatment to obtain Spiro-OMeTAD; the light wavelength is 400 to 780 nm, and the intensity is 1000 to 30000 Lux.

[0030] In the above embodiment, the specific active sites of the photosensitive catalyst can provide better chemical substitution selectivity in the process of generating Spiro-OMeTAD, reduce the generation of Spiro-OMeTAD isomer impurities, and obtain Spiro-OMeTAD with higher conversion rate and purity; in addition, the Spiro-OMeTAD molecules can be oxidized synchronously during the photocatalytic reaction to form Spiro-OMeTAD oxidized state molecules without lithium salt doping and high conductivity, which can effectively avoid the influence of lithium salt moisture absorption and ion migration on the performance of the corresponding photoelectric device. The preparation method can significantly shorten the preparation cycle of oxidized Spiro-OMeTAD, reduce the preparation cost, and accelerate the application process of Spiro-OMeTAD molecules.

[0031] In a preferred embodiment, the illumination conditions preferably have a wavelength of 400 nm, an intensity of 30,000 Lux and an illumination duration of 1 h, which has a higher conversion rate and a lower isomer content.

[0032] In a preferred embodiment, the molar ratio between the 4,4'-dimethoxydiphenylamine and the 2,2',7,7'-tetrabromo-9,9'-spirobifluorene is (1-4):1.

[0033] In a preferred embodiment, the photosensitive catalyst is selected from titanium dioxide, Ru(bpy)3Cl2, Co(bpy)3C l2 , Fe(bpy)3Cl2, single-atom palladium, PhCH(CN)2, Ir(ppy)2(dtbbpy)(PF6), more preferably Co(bpy)3C l2 ; and / or, the molar amount of the photosensitive catalyst is 0.01-0.1% of the total molar amount of the reaction substrate.

[0034] In a preferred embodiment, the ligand is selected from one of 1,1'-binaphthyl-2,2'-bisdiphenylphosphine, 4,5-bisdiphenylphosphine-9,9-dimethylxanthene, 1,1'-bis(diphenylphosphino)ferrocene, tri-tert-butylphosphine, and tri-tert-butylphosphine tetrafluoroboric acid; preferably, the safer tri-tert-butylphosphine tetrafluoroboric acid.

[0035] In a preferred embodiment, the organic solvent is selected from commonly used organic solvents such as tetrahydrofuran or toluene.

[0036] In a preferred embodiment, step a) is carried out under an inert atmosphere, and the reagent is added to the solvent and stirred to dissolve under the protection of an inert gas to prevent the reagent from being oxidized and ineffective. The inert atmosphere is stopped before the light irradiation, that is, in step b), the reactor is kept stirring and reacting normally, and the reaction liquid surface is kept connected to the outside air to introduce oxygen, and the Spiro-OMeTAD is catalyzed to generate and oxidized to obtain highly conductive Spiro-OMeTAD oxidized molecules under light conditions.

[0037] Example 1

[0038] 1.5mmol of 4,4'-dimethoxydiphenylamine, 0.5mmol of 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 1.5mmol of potassium tert-butoxide, 0.1% of photosensitive catalyst Co(bpy)3Cl2, and 0.1mmol of tri-tert-butylphosphine tetrafluoroborate were added to a 100mL completely dried three-necked flask, and argon was introduced for 1h, and then 50mL of anhydrous toluene was added as solvent. Stir at room temperature for 1h under the protection of inert gas until the raw materials are completely dissolved, and then remove the inert gas. Apply 500nm visible light with an intensity of 20000Lux above the reactor and illuminate for 1h. After the reaction is completed, wait for the solution to cool, transfer it to a single-necked bottle, and concentrate the reaction solution by rotary evaporation to obtain a black oily substance. The oily substance was acid-washed several times, the organic phase was collected, and a white solid was obtained by rotary drying. The product was identified as Spiro-OMeTAD by infrared spectroscopy.

[0039] Example 2

[0040] 1.5mmol of 4,4'-dimethoxydiphenylamine, 0.5mmol of 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 1.5mmol of potassium tert-butoxide, 0.1% of the photosensitive catalyst Co(bpy)3Cl2, and 0.1mmol of 1,1'-bis(diphenylphosphino)ferrocene were added to a 100mL completely dried three-necked flask, and argon was introduced for 1h, and then 50mL of anhydrous toluene was added as a solvent. Stir at room temperature for 1h under the protection of inert gas until the raw materials are completely dissolved, and then remove the inert gas. Apply 780nm visible light with an intensity of 30000Lux above the reactor and illuminate for 1h. After the reaction is completed, wait for the solution to cool, transfer it to a single-necked bottle, and concentrate the reaction solution by rotary evaporation to obtain a black oily substance. The oily substance was acid-washed several times, the organic phase was collected, and the white solid was obtained by rotary drying. The product was identified as Spiro-OMeTAD by infrared spectroscopy.

[0041] Example 3

[0042] 1.5mmol of 4,4'-dimethoxydiphenylamine, 0.5mmol of 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 1.5mmol of potassium tert-butoxide, 0.1% of the photosensitive catalyst Co(bpy)3Cl2, and 0.1mmol of tri-tert-butylphosphine tetrafluoroborate were added to a 100mL completely dried three-necked flask, and argon was introduced for 1h, and then 50mL of tetrahydrofuran was added as a solvent. Stir at room temperature for 1h under the protection of inert gas until the raw materials are completely dissolved, and then remove the inert gas. Apply 400nm visible light with an intensity of 30000Lux above the reactor and illuminate for 1h. After the reaction is completed, wait for the solution to cool, transfer it to a single-necked flask, and concentrate the reaction solution by rotary evaporation to obtain a black oily substance. The oily substance was acid-washed several times, the organic phase was collected, and a white solid was obtained by rotary drying. The product was identified as Spiro-OMeTAD by infrared spectroscopy.

[0043] Example 4

[0044] 2mmol of 4,4'-dimethoxydiphenylamine, 0.5mmol of 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 1.5mmol of potassium tert-butoxide, 0.05% of the photosensitive catalyst Co(bpy)3Cl2, and 0.1mmol of tri-tert-butylphosphine tetrafluoroborate were added to a 100mL completely dried three-necked flask, and argon was introduced for 1h, and then 50mL of tetrahydrofuran was added as a solvent. Stir at room temperature for 1h under the protection of inert gas until the raw materials are completely dissolved, and then remove the inert gas. Apply 400nm visible light with an intensity of 10000Lux above the reactor and illuminate for 5h. After the reaction is completed, wait for the solution to cool, transfer it to a single-necked flask, and concentrate the reaction solution by rotary evaporation to obtain a black oily substance. The oily substance was acid-washed several times, the organic phase was collected, and the white solid was obtained by rotary drying. The product was identified as Spiro-OMeTAD by infrared spectroscopy.

[0045] Example 5

[0046] 0.5mmol of 4,4'-dimethoxydiphenylamine, 0.5mmol of 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 1.5mmol of potassium tert-butoxide, 0.1% of photosensitive catalyst Co(bpy)3Cl2, and 0.1mmol of tri-tert-butylphosphine tetrafluoroborate were added to a 100mL completely dried three-necked flask, and argon was introduced for 1h, and then 50mL of anhydrous toluene was added as solvent. Stir at room temperature for 1h under the protection of inert gas until the raw materials are completely dissolved, and then remove the inert gas. Apply 400nm visible light with an intensity of 30000Lux above the reactor and illuminate for 24h. After the reaction is completed, wait for the solution to cool, transfer it to a single-necked bottle, and concentrate the reaction solution by rotary evaporation to obtain a black oily substance. The oily substance was acid-washed several times, the organic phase was collected, and the white solid was obtained by rotary drying. The product was identified as Spiro-OMeTAD by infrared spectroscopy.

[0047] Example 6

[0048] 2.0mmol of 4,4'-dimethoxydiphenylamine, 0.5mmol of 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 1.5mmol of potassium tert-butoxide, 0.05% of the photosensitive catalyst Co(bpy)3Cl2, and 0.1mmol of tri-tert-butylphosphine tetrafluoroborate were added to a 100mL completely dried three-necked flask, and after passing argon for 1h, 50mL of anhydrous toluene was added as a solvent. Stir at room temperature for 1h under the protection of inert gas until the raw materials are completely dissolved and then remove the inert gas. Apply 400nm visible light with an intensity of 30000Lux above the reactor and illuminate for 48h. After the reaction is completed, wait for the solution to cool, transfer it to a single-necked flask, and concentrate the reaction solution by rotary evaporation to obtain a black oily substance. The oily substance was acid-washed several times, the organic phase was collected, and the white solid was obtained by rotary drying. The product was identified as Spiro-OMeTAD by infrared spectroscopy.

[0049] Comparative Example 1

[0050] Add 2.0mmol of 4,4'-dimethoxydiphenylamine, 0.5mmol of 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 1.5mmol of potassium tert-butoxide, 0.1% of palladium acetate, and 0.1mmol of tri-tert-butylphosphine tetrafluoroborate to a 100mL completely dried three-necked flask, pass argon for 1h, and then add 50mL of anhydrous toluene as solvent. Stir at room temperature for 1h under the protection of inert gas until the raw materials are completely dissolved, and then heat and reflux overnight for 12h. After the reaction is completed, wait for the solution to cool, transfer it to a single-necked flask, and concentrate the reaction solution by rotary evaporation to obtain a black oily substance. The oily substance is acid-washed several times, the organic phase is collected, and the white solid is obtained by rotary drying.

[0051] Experimental Example 1

[0052] The composition and purity of the products in the above embodiments and comparative examples were tested by GC-MS, and the conductivity of the products was characterized by a conductivity meter. The results are shown in Table 1.

[0053] Table 1:

[0054]

[0055] It is not difficult to see from Table 1 that the isomer content in the products obtained in Examples 1-6 is controlled below 5%, and the conversion rate is above 90%, which is significantly higher than the conventional catalytic method used in the prior art. The conversion rate obtained by using the conventional catalytic method in Comparative Example 1 is low, and the product contains a large amount of isomers. The conductivity in Comparative Example 1 is only 10 -7 S / cm level, while in Examples 1-6 it reached 10 -3 S / cm level, indicating the production of oxidized Spiro-OMeTAD and a significant increase in conductivity.

[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. Photocatalytic synthesis of Spiro-OMeTAD, It is characterized in that the steps include: a) dissolving 2,2',7,7'-tetrabromo-9,9'-spirobifluorene, 4,4'-dimethoxydiphenylamine, alkali metal alkoxide, photosensitive catalyst and ligand in an organic solvent and stirring uniformly; b) applying light to the solution system of step a) for 1 to 48 hours, and then performing post-treatment to obtain Spiro-OMeTAD; the light wavelength is 400 to 780 nm, and the intensity is 1000 to 30000 Lux.

2. The photocatalytic synthesis method according to claim 1, It is characterized in that The illumination conditions are: wavelength 400nm, intensity 30000Lux, and illumination duration 1h.

3. The photocatalytic synthesis method according to claim 1, It is characterized in that The molar ratio between the 4,4'-dimethoxydiphenylamine and the 2,2',7,7'-tetrabromo-9,9'-spirobifluorene is (1-4):

1.

4. The photocatalytic synthesis method according to claim 1, It is characterized in that The photosensitive catalyst is selected from titanium dioxide, Ru(bpy) 3 Cl 2 、Co(bpy) 3 C l2 、Fe(bpy) 3 Cl 2 , single-atom palladium, PhCH(CN) 2 、Ir(ppy) 2 (dtbbpy)(PF 6 ) or more thereof; and / or, the molar amount of the photosensitive catalyst is 0.01-0.1% of the total molar amount of the reaction substrate.

5. The photocatalytic synthesis method according to claim 1, It is characterized in that The ligand is selected from one of 1,1'-binaphthyl-2,2'-bisdiphenylphosphine, 4,5-bisdiphenylphosphine-9,9-dimethylxanthene, 1,1'-bis(diphenylphosphino)ferrocene, tri-tert-butylphosphine, and tri-tert-butylphosphine tetrafluoroborate.

6. The photocatalytic synthesis method according to claim 1, It is characterized in that The organic solvent is selected from tetrahydrofuran or toluene.

7. The photocatalytic synthesis method according to claim 1, It is characterized in that Step a) is carried out under an inert atmosphere.

8. Spiro-OMeTAD obtained by the photocatalytic synthesis method according to any one of claims 1 to 7.

9. The Spiro-OMeTAD according to claim 8, It is characterized in that Its conductivity is greater than 1.0×10 -4 S / cm.

10. Solar cells, It is characterized in that It comprises a hole transport layer and a perovskite layer; the hole transport layer comprises the Spiro-OMeTAD according to any one of claims 8 to 9.