Imidazole compound, organic electroluminescent device and display device

By designing imidazole compounds as luminescent layer materials of organic electroluminescent devices, the problems of insufficient efficiency and stability in the existing technology are solved, and organic electroluminescent devices with low driving voltage and high current efficiency are realized.

CN118724876APending Publication Date: 2024-10-01FUYANG SINEVA MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410678448.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing organic electroluminescent materials have problems with insufficient efficiency and stability in practical applications, especially in terms of driving voltage and current efficiency. There is room for improvement.

Method used

An imidazole compound is designed, which has excellent luminescence properties and good thermal stability, and is used as a light-emitting layer material in organic electroluminescent devices to reduce driving voltage and improve current efficiency through structural design.

Benefits of technology

It effectively reduces the driving voltage of the organic electroluminescent device, improves its current efficiency, and enhances the luminescence performance, and is suitable for high-efficiency organic electroluminescent device applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004864900650000011
    Figure BDA0004864900650000011
  • Figure BDA0004864900650000022
    Figure BDA0004864900650000022
  • Figure BDA0004864900650000041
    Figure BDA0004864900650000041
Patent Text Reader

Abstract

The invention provides an imidazole compound, an organic electroluminescent device and a display device, and relates to the technical field of organic photoelectric display. The imidazole compound has a structure as shown in a formula I and a formula II. By designing the structure of the imidazole compound, the obtained imidazole compound has good thermal stability and excellent luminescence performance, can be used for preparing the organic electroluminescent device, especially can be used as a luminescent layer material in the organic electroluminescent device, and can effectively reduce the driving voltage of the organic electroluminescent device and improve the luminous efficiency of the organic electroluminescent device. And the current efficiency of the organic electroluminescent device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of organic photoelectric display, and in particular relates to an imidazole compound, an organic electroluminescent device and a display device. Background Art

[0002] Organic light emitting diodes (OLEDs) are display components that utilize the phenomenon of self-luminescence and have a wide viewing angle. Compared with liquid crystal display components, OLED components are thinner and lighter, have a faster response speed, and can achieve flexible displays. Therefore, their application as full-color display components or lighting equipment is highly anticipated.

[0003] Generally, the organic light-emitting phenomenon refers to the phenomenon of converting electrical energy into light energy using organic substances. An organic light-emitting element generally has a structure including an anode, a cathode, and an organic layer sandwiched between the anode and the cathode. In order to improve the efficiency and stability of the organic light-emitting element, the organic layer is composed of a multilayer structure composed of different substances in most cases, for example, it can be composed of a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, etc. If a voltage is applied between the two electrodes in the structure of such an organic light-emitting element, the holes in the anode will be injected into the organic layer, and the electrons in the cathode will also be injected into the organic layer. When the injected holes and electrons meet, excitons are formed. When the exciton releases energy and transitions to the ground state, photons will be emitted, thereby generating light. Such an organic light-emitting element is widely believed to have the characteristics of self-luminescence, high brightness, high efficiency, low driving voltage, wide viewing angle, high contrast, and high-speed responsiveness.

[0004] At present, the research on organic electroluminescent materials has been widely carried out in academia and industry. Designing and finding a compound as a new material for the OLED light-emitting layer to overcome its shortcomings in practical applications is a technical problem that OLED material technicians urgently need to solve. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an imidazole compound, an organic electroluminescent device and a display device. The imidazole compound of the present invention has excellent luminescent properties and is suitable for use as a luminescent layer material in an organic electroluminescent device.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides an imidazole compound having a structure shown in the following formula I and formula II:

[0008]

[0009] Wherein, X is selected from a single bond, O, S, Se,

[0010] L is selected from substituted or unsubstituted C6~C 30 Aromatic hydrocarbon or C3~C 30 The aromatic heterocyclic group is preferably selected from the following structures:

[0011]

[0012] R1, R2, R3, R4, and R5 are each independently selected from substituted or unsubstituted C1 to C 12 Alkyl or substituted or unsubstituted C6~C 30 Aromatic hydrocarbon or C3~C 30 An aromatic heterocyclic group;

[0013] The substituents of each of R1, R2, R3, R4 and R5 are selected from at least one of a deuterium atom, F, CN, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-pentyl group, a tert-pentyl group, an n-hexyl group, a cyclohexyl group, a phenylene group, a biphenylene group, a terphenylene group, a naphthyl group, an anthrylene group, an indenyl group, a fluorenyl group, a perylene group, a phenanthrenyl group, a pyrenyl group, a fluoranthenyl group, a spirofluorenyl group or a phenylene group, a benzofuranyl group, a benzothienyl group, a dibenzofuranyl group, a dibenzothienyl group, a carbazolyl group, a diarylamine group, a benzofuranocarbazolyl group, a benzofuranothienyl group, a triazinyl group and a pyridyl group;

[0014] All hydrogen atoms in the compounds of formula I and formula II can be replaced independently by deuterium atoms, F, CN, C1-C 12 Alkyl or C6~C 30 Aryl or C3~C 30 A kind of aromatic heterocyclic group is substituted;

[0015] * indicates the attachment site.

[0016] The imidazole compounds obtained by structural design in the present invention have good thermal stability and excellent luminescent properties, and can be used to prepare organic electroluminescent devices, especially as light-emitting layer materials in organic electroluminescent devices, which can effectively reduce the driving voltage of organic electroluminescent devices and improve the current efficiency of organic electroluminescent devices.

[0017] In the present invention, the C1 to C 12 The alkyl groups are each independently selected from one of methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl, tert-pentyl, n-hexyl, cyclohexyl, etc.;

[0018] C6~C 30The aromatic hydrocarbon group is a general term for a monovalent group remaining after removing a hydrogen atom from the aromatic carbon nucleus of an aromatic hydrocarbon molecule, which may be a monocyclic aromatic group or a condensed aromatic group, and illustratively includes but is not limited to: phenyl, biphenyl, terphenyl, naphthyl, anthracenyl, indenyl, fluorenyl, perylenyl, phenanthrenyl, pyrenyl, fluoranthenyl or triphenylenyl, etc.;

[0019] C3~C 30 The aromatic heterocyclic group refers to a general term for groups in which one or more aromatic carbon atoms in an aromatic group are replaced by heteroatoms, wherein the heteroatoms include but are not limited to oxygen, sulfur and nitrogen atoms, and the heteroaryl group may be a monocyclic heteroaryl group or a condensed-ring heteroaryl group, and illustratively include but are not limited to: benzofuran, benzothiophene, dibenzofuran, dibenzothiophene, carbazole, benzofurancarbazole, benzofuranthiophene, and triazine.

[0020] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0021] C1~C 12 The alkyl group is preferably one of methyl, ethyl and tert-butyl;

[0022] C6~C 30 The aromatic hydrocarbon group is preferably one of phenyl, biphenyl, naphthyl and terphenyl;

[0023] C3~C 30 The aromatic heterocyclic group is preferably one of dibenzofuran, dibenzothiophene or carbazole;

[0024] As a preferred technical solution of the present invention, the imidazole compound includes any one of the following compounds:

[0025]

[0026]

[0027]

[0028]

[0029]

[0030]

[0031]

[0032]

[0033]

[0034]

[0035]

[0036]

[0037] Preferably, the compound represented by Formula I or Formula II is selected from any one of Compounds 1 to 28:

[0038]

[0039] The present invention lists some specific structural forms of the imidazole compounds, but the imidazole compounds of the present invention are not limited to these listed chemical structures. All structures based on the structures shown in Formula I and Formula II, in which X, L, R1, R2, R3, R4, and R5 meet the above-mentioned limiting conditions should be included.

[0040] In a second aspect, the present invention provides an intermediate for preparing the imidazole compound of the present invention, having the following structure:

[0041]

[0042]

[0043] In a third aspect, the present invention provides an organic electroluminescent device, wherein the organic electroluminescent device comprises the imidazole compound described in the first aspect.

[0044] Preferably, the organic electroluminescent device comprises a first electrode, a second electrode and an organic layer disposed between the first electrode and the second electrode; the material of the organic layer comprises the imidazole compound described in the first aspect.

[0045] Preferably, the organic layer comprises a light-emitting layer;

[0046] Preferably, the light-emitting layer is prepared by a solution method;

[0047] The material of the light-emitting layer includes the imidazole compound described in the first aspect.

[0048] In a fourth aspect, the present invention provides a display device, comprising the organic electroluminescent device described in the third aspect.

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] The present invention provides an imidazole compound, an organic electroluminescent device and a display device. By designing the structure of the imidazole compound, the obtained imidazole compound has good thermal stability and luminescent performance, can be used to prepare the organic electroluminescent device, especially as a light-emitting layer material in the organic electroluminescent device, can effectively reduce the driving voltage of the organic electroluminescent device and improve the current efficiency of the organic electroluminescent device. DETAILED DESCRIPTION

[0051] For the convenience of understanding the present invention, the present invention lists the preparation examples and embodiments as follows. It should be understood by those skilled in the art that the preparation examples and embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0052] Preparation Example 1

[0053] This preparation example provides a method for synthesizing intermediate 10 and intermediate 10B, as described below:

[0054]

[0055] 0.1 mol of bromide 10 was dissolved in 200 mL of THF, and then cooled to -78°C under nitrogen protection. 0.105 mol of n-butyl lithium (2.5 M, 42 ml) was added dropwise. After the addition was completed, the temperature was kept warm for 1 hour. Then 0.2 mol of DMF was added dropwise. After the addition was completed, the temperature was kept warm for 1 hour. Then the temperature was slowly raised to room temperature. The gas phase was sampled and sent for inspection. Aldehyde 1: Aldehyde 2 = 95:2. Water was added to quench the reaction. The liquids were separated. The aqueous phase was extracted once with toluene and then combined with the organic phase. The organic phase was concentrated and dried, and then passed through a column with n-heptane and dichloromethane = 10:1 to separate the intermediate aldehyde 1.

[0056] 0.1 mol of benzil, 0.1 mol of 3-trifluoromethylaniline, and 0.1 mol of aldehyde 1 were added to a reaction bottle, and 0.2 mol of ammonium acetate and 300 ml of acetic acid were added. The temperature was raised to 130°C under nitrogen protection and the reaction was kept for 24 hours. After the reaction was completed, the temperature was lowered to room temperature, 800 ml of water was added to precipitate the solid, and the crude product was directly filtered out. The crude product was recrystallized with a mixed solvent of toluene and ethanol (volume ratio of 1:1) to obtain intermediate 10.

[0057] The mass spectrum data of intermediate 10 was tested, and the mass spectrum m / z was measured to be 683.1. The measured element content (%) was: C, 70.15; H, 3.70; Br, 11.67; F, 8.33; N, 6.15.

[0058] Take 0.01 mol of intermediate 10, 0.015 mol of pinacol borate, 0.03 mol of potassium acetate, 0.0001 mol of bis(triphenylphosphine)palladium dichloride, and 50 ml of toluene, heat to 110°C and reflux for 8 h, add 50 ml of water, separate the liquids while hot, cool the organic phase to 25°C, and directly filter to obtain intermediate 10B.

[0059] The mass spectrometry test of intermediate 10B showed that the mass spectrum m / z was 731.3. The measured element contents (%) were: C, 75.52; H, 5.12; B, 1.45; F, 7.80; N, 5.74.

[0060] Referring to Preparation Example 1, the bromide 10 in Preparation Example 1 was replaced by the bromide in the following table, and other conditions remained unchanged to obtain the following intermediates, as shown in Table 1.

[0061] Table 1 Bromo compounds and prepared intermediates of Preparation Examples 2-13

[0062]

[0063]

[0064] Preparation Example 14

[0065] This preparation example provides a method for synthesizing intermediate 23 and intermediate 23B, as described below:

[0066]

[0067] 0.1 mol of 9,10-phenanthrenedione, 0.1 mol of 3-trifluoromethylaniline, and 0.1 mol of aldehyde 1 (prepared by the same method as in Preparation Example 1) were added to a reaction bottle, and 0.2 mol of ammonium acetate and 300 ml of acetic acid were added. The temperature was raised to 130°C under nitrogen protection and the reaction was kept for 24 hours. After the reaction was completed, the temperature was lowered to room temperature, 800 ml of water was added to precipitate the solid, and the crude product was directly filtered out. The crude product was recrystallized with a mixed solvent of toluene and ethanol (volume ratio of 1:1) to obtain intermediate 23.

[0068] The mass spectrum data of intermediate 23 was tested, and the mass spectrum m / z was measured to be 681.1.

[0069] Take 0.01 mol of intermediate 23, 0.015 mol of pinacol borate, 0.03 mol of potassium acetate, 0.0001 mol of bis(triphenylphosphine)palladium dichloride, and 50 ml of toluene, heat to 110°C and reflux for 8 h, add 50 ml of water, separate the liquids while hot, cool the organic phase to 25°C, and directly filter to obtain intermediate 23B.

[0070] The intermediate 23B was subjected to mass spectrometry and the mass spectrum m / z was measured to be 729.3.

[0071] Referring to Preparation Example 14, the bromide 10 in Preparation Example 14 was replaced by the bromide in the following table, and other conditions remained unchanged to obtain the following intermediates, as shown in Table 2.

[0072] Table 2 Bromo compounds of Preparation Examples 15-26 and prepared intermediates

[0073]

[0074]

[0075] Synthesis Example 1

[0076] This embodiment provides a method for synthesizing compound 1, as described below:

[0077]

[0078] 0.1 mol of carbazole, 0.12 mol of bromide a, 0.2 mol of potassium carbonate, 0.01 mol of cuprous iodide and 500 mL of DMF solvent were heated under reflux for 24 h under nitrogen protection. After the reaction was completed, the reaction solution was naturally cooled to room temperature, poured into water, extracted with 3×200 mL of toluene, the organic phases were combined, dried with anhydrous magnesium sulfate, filtered under reduced pressure to remove anhydrous magnesium sulfate, and then concentrated to obtain a crude product. Silica gel was used as the stationary phase, and after toluene was passed through the column, the crude product was recrystallized with toluene and ethanol (volume ratio 1:1) to obtain compound 1.

[0079] The mass spectrum data of compound 1 was tested, and the mass spectrum m / z was measured to be 605.2.

[0080] Synthesis Example 2

[0081] This embodiment provides a method for synthesizing compound 2, as described below:

[0082]

[0083] 0.01mol of boric acid 1, 0.01mol of bromide 1, 0.02mol of potassium carbonate, 0.0005mol of tetrakis(triphenylphosphine)palladium, 50mL of toluene, 20ml of ethanol, and 20ml of water were added to the reaction bottle, and heated under reflux for 8h under nitrogen protection. After the reaction was completed, the reaction solution was naturally cooled to room temperature, and then directly filtered to obtain a crude product, which was heated and dissolved in toluene and then passed through a silica gel column. The column liquid was concentrated and recrystallized with a mixed solution of toluene and ethanol (volume ratio of 2:1) to obtain compound 2.

[0084] The mass spectrum data of compound 2 was tested and the mass spectrum m / z was measured to be 681.2.

[0085] Synthesis Example 3

[0086] This embodiment provides a method for synthesizing compound 6, as follows:

[0087]

[0088] 0.1 mol of carbazole, 0.12 mol of intermediate 10, 0.2 mol of potassium carbonate, 0.01 mol of cuprous iodide, and 600 mL of DMF solvent were heated to reflux for 16 h under nitrogen protection. After the reaction was completed, the reaction solution was naturally cooled to room temperature, poured into water, extracted with 3×200 mL of toluene, the organic phases were combined, dried with anhydrous magnesium sulfate, filtered under reduced pressure to remove anhydrous magnesium sulfate, and then concentrated to obtain a crude product, which was purified by column chromatography using silica gel as the stationary phase and a mixed solvent of n-heptane and DCM (volume ratio 1:1) as the eluent to obtain compound 6.

[0089] The mass spectrum data of compound 6 was tested and the mass spectrum m / z was measured to be 770.3.

[0090] Synthesis Example 4

[0091] This embodiment provides a method for synthesizing compound 13, as described below:

[0092]

[0093] 0.01 mol of intermediate 22B, 0.01 mol of bromide b, 0.02 mol of potassium carbonate, 0.0005 mol of tetrakis(triphenylphosphine)palladium, 80 mL of toluene, 40 ml of ethanol, and 40 ml of water were added to a reaction flask, and heated to reflux for 12 h under nitrogen protection. After the reaction was completed, the reaction solution was naturally cooled to room temperature, and then directly filtered to obtain a crude product, which was heated and dissolved in toluene and then passed through a silica gel column. The column liquid was concentrated to dryness and recrystallized with toluene to obtain compound 13.

[0094] The mass spectrum data of compound 13 was tested, and the mass spectrum m / z was measured to be 831.3.

[0095] Other intermediates and compounds whose specific synthesis steps are not listed can be prepared by common knowledge in the art in combination with the above embodiments.

[0096] The specific structures of the compounds used in the following device examples and device comparative examples are shown below:

[0097]

[0098] In the following device examples, the imidazole compounds provided by the present invention are selected as the light-emitting layer doping materials in the organic electroluminescent device, and in the device comparative examples, the above-mentioned BD-1 and BD-2 are selected as the light-emitting layer doping materials in the organic electroluminescent device.

[0099] Device Example 1

[0100] This device embodiment provides an organic electroluminescent device, using the compound 1 provided in Synthesis Example 1 of the present invention as a doping material for the light-emitting layer; and in this embodiment, the light-emitting layer is prepared by a solution method.

[0101] The structure of the organic electroluminescent device is:

[0102] ITO / HT (40 nm) / BH-1: Compound 13% / TPBI (30 nm) / LiF (0.5 nm) / Al (150 nm).

[0103] The preparation method of the organic electroluminescent device is as follows:

[0104] The glass substrate coated with an ITO transparent conductive layer (as an anode) is ultrasonically treated in a cleaning agent, then rinsed in deionized water, ultrasonically degreased in a mixed solvent of acetone and ethanol, baked in a clean environment until the water is completely removed, cleaned with ultraviolet light and ozone, and bombarded with a low-energy cation beam to improve the properties of the surface and enhance the binding ability with the hole injection layer;

[0105] The glass substrate was placed in a vacuum chamber and evacuated to 1×10 -5 ~9×10 -3 Pa, HT was vacuum evaporated on the anode as a hole transport layer, the evaporation rate was 0.1nm / s, and the evaporation film thickness was 40nm;

[0106] The glass substrate on which the hole transport layer has been evaporated was transferred to a glove box filled with nitrogen, and a solution of BH-1 and 3% by mass of the compound described in this patent or BH-1 and 3% by mass of the comparative compound in 4-cyclohexylbenzene:chlorobenzene = 3:1 (volume ratio) was spin-coated on the hole transport layer, respectively, at a spin coating speed of 1000 rpm for 60 seconds, and then the glass substrate was heated at 80°C for 2 hours, and the solvent was removed in vacuo. By adjusting the concentrations of BH-1 and the compound of the present invention in the solvent and the concentrations of BH-1 and the comparative compound in the solvent, the thickness of the obtained light-emitting layer was about 30 to 40 nm, as shown in Table 1 (the unit of the light-emitting layer thickness is nm).

[0107] The glass substrate on which the light-emitting layer has been spin-coated in the previous step is transferred into a vacuum chamber, and TPBI is vacuum-evaporated on the light-emitting layer as the electron transport layer of the device. The evaporation rate is 0.1 nm / s, and the total evaporation film thickness is 30 nm;

[0108] 0.5 nm of LiF and 150 nm of Al were vacuum-deposited on the electron transport layer to serve as an electron injection layer and a cathode.

[0109] The brightness, driving voltage and current efficiency of the prepared organic electroluminescent device were measured.

[0110] Device Examples 2-20

[0111] Device Examples 2-20 respectively provide an organic electroluminescent device, which differs from Device Example 1 only in that the doping materials of the light-emitting layer are different (see Table 3 below for details), and other conditions are the same as those of Device Example 1.

[0112] Device Comparison Example 1-2

[0113] Device Comparative Examples 1-2 respectively provide an organic electroluminescent device, which differs from Device Example 1 only in that the doping materials of the light-emitting layer are different (see Table 3 below for details), and other conditions are the same as those of Device Example 1.

[0114] Performance Testing

[0115] Test the driving voltage, current efficiency and life LT90 of the OLED devices provided above; LT90 refers to the time required for the brightness to drop to 90% of the original brightness while maintaining the current density at the initial brightness of 1000nit. The test items include the brightness, driving voltage and current efficiency of the organic electroluminescent device. The driving voltage, current efficiency and LT90 data are all based on a brightness of 1000cd / m 2 The relative value of the organic electroluminescent device performance test results are shown in Table 3 below:

[0116] Table 3 Device Examples 1-20, Device Comparative Examples 1-2 Light-emitting layer doping materials and organic electroluminescent device performance test results

[0117]

[0118]

[0119] It can be seen from the contents of Table 3 that the present invention obtains imidazole compounds through molecular design. The imidazole compounds provided by the present invention can be used as doping materials for the light-emitting layer of an OLED light-emitting device, so that the OLED light-emitting device has a lower driving voltage, higher current efficiency and longer life.

[0120] The present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An imidazole compound, characterized in that The imidazole compound has the structure shown in the following formula I and formula II: Wherein, X is selected from a single bond, O, S, Se, L is selected from substituted or unsubstituted C6~C 30 Aromatic hydrocarbon or C3~C 30 An aromatic heterocyclic group; R1, R2, R3, R4, and R5 are each independently selected from substituted or unsubstituted C1 to C 12 Alkyl or substituted or unsubstituted C6~C 30 Aromatic hydrocarbon or C3~C 30 An aromatic heterocyclic group; The substituents of each of R1, R2, R3, R4 and R5 are selected from at least one of a deuterium atom, F, CN, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-pentyl group, a tert-pentyl group, an n-hexyl group, a cyclohexyl group, a phenylene group, a biphenylene group, a terphenylene group, a naphthyl group, an anthrylene group, an indenyl group, a fluorenyl group, a perylene group, a phenanthrenyl group, a pyrenyl group, a fluoranthenyl group, a spirofluorenyl group or a phenylene group, a benzofuranyl group, a benzothienyl group, a dibenzofuranyl group, a dibenzothienyl group, a carbazolyl group, a diarylamine group, a benzofuranocarbazolyl group, a benzofuranothienyl group, a triazinyl group and a pyridyl group; All hydrogen atoms in the compounds of formula I and formula II can be replaced independently by deuterium atoms, F, CN, C1-C 12 Alkyl or C6~C 30 Aromatic hydrocarbon or C3~C 30 A substituted aromatic heterocyclic group.

2. The imidazole compound according to claim 1, characterized in that The L is selected from any one of the following structures:

3. The imidazole compound according to claim 1, characterized in that C1~C 12 The alkyl groups are each independently selected from any one of methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl, tert-pentyl, n-hexyl and cyclohexyl.

4. The imidazole compound according to claim 1, characterized in that C3~C 30 The heteroatom in the aromatic heterocyclic group is selected from one of oxygen, sulfur, selenium, nitrogen and silicon.

5. The imidazole compound according to claim 4, characterized in that C3~C 30 The aromatic heterocyclic group is selected from one of benzofuran, benzothiophene, dibenzofuran, dibenzothiophene, carbazole, benzofuranocarbazole, benzofuranothiophene and triazine.

6. The imidazole compound according to any one of claims 1 to 5, characterized in that The compound is selected from any one of the following compounds:

7. An organic electroluminescent device, characterized in that: The organic electroluminescent device comprises the imidazole compound according to claim 1.

8. The organic electroluminescent device according to claim 7, characterized in that: The organic electroluminescent device comprises a first electrode, a second electrode and an organic layer disposed between the first electrode and the second electrode; The material of the organic layer includes the imidazole compound according to claim 1.

9. The organic electroluminescent device according to claim 8, characterized in that: The organic layer includes a light-emitting layer; the material of the light-emitting layer includes the imidazole compound according to claim 1.

10. A display device, characterized in that: The display device comprises the organic electroluminescent device according to any one of claims 7 to 9.