Leveling agent for powder coating as well as preparation method and application of leveling agent

Through the preparation of modified leveling agents, fluorine-containing silane coupling agents and epoxy phosphates are used to modify nano-silica and polyacrylate to form a three-dimensional network structure, which solves the problem in the drying process of polyacrylate leveling agents. The problem of surface defects improves the adhesion and leveling effect of the coating.

CN118725213APending Publication Date: 2024-10-01浙江双彩新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410934642.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing polyacrylate leveling agents are prone to surface defects such as blooming, orange peel, shrinkage holes, and pinholes during the drying process, which affects the adhesion strength and protective performance of the coating.

Method used

By using fluorine-containing silane coupling agents to modify nano-silica, and introducing epoxy phosphate and polyacrylate molecular segments for modification, a three-dimensional network structure is formed to improve the compatibility and cross-linking density of the leveling agent. , reduce fine pores and improve the smoothness and uniformity of the coating surface.

Benefits of technology

It effectively avoids blooming, orange peel, shrinkage holes and pinhole defects on the surface of the coating film, improves the adhesion and flow rate of the coating, and enhances the leveling effect and adhesion performance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725213A_ABST
    Figure CN118725213A_ABST
Patent Text Reader

Abstract

The invention provides a leveling agent for a powder coating and a preparation method and application thereof, and belongs to the technical field of powder paints.The preparation method of the leveling agent for the powder coating comprises the steps that S1, 30 parts by weight of acrylic ester and 0.2-0.5 part by weight of glycidyl methacrylate are added into a reaction kettle and stirred to be uniform, the temperature is increased to 70-80 DEG C, and the mixture is stirred to be uniform; the preparation method comprises the following steps: weighing 40-50 parts of deionized water and 0.5-1.5 parts of tert-butyl peroxybenzoate, dropwise adding the deionized water and the tert-butyl peroxybenzoate into a reaction kettle for 0.5-1.5 hours, and after the deionized water and the tert-butyl peroxybenzoate are dropwise added, carrying out constant-temperature reaction for 0.5-1.5 hours; s2, adding 4-8 parts of modified silicon dioxide into the reaction kettle, cooling to 50-60 DEG C, and stirring at a high speed for 2-3 hours to obtain a polyacrylate emulsion; s3, in a stirring state, adding 8-12 parts of epoxy phosphate into the polyacrylate emulsion obtained in the step S2, continuously stirring, reacting for 2-5 hours, naturally cooling to room temperature, adjusting the pH to 7-8 by using ammonia water, and filtering to obtain the water-based paint. According to the invention, high leveling level is guaranteed, and coating surface defects such as floating, orange peel, shrinkage cavities and needle holes are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder coatings, and in particular relates to a leveling agent for powder coatings and a preparation method and application thereof. Background Art

[0002] Powder coating is a solid powder coating composed of resin, pigment, filler and additives. Unlike conventional coatings, powder coating does not use solvents during use and has the characteristics of economy, environmental protection, safety, harmlessness and high efficiency. Leveling agent is a common additive in powder coating, which can reduce the surface tension of the coating liquid, improve the permeability of the coating liquid, and make the coating form a smooth coating film during the film forming process.

[0003] There are two main types of leveling agents in powder coatings: polyacrylates and polysiloxanes. Compared with polysiloxane leveling agents, polyacrylate leveling agents are less sensitive to overuse and contamination, and can balance the difference in surface tension of the paint film, thereby obtaining a truly smooth paint film surface. Therefore, polyacrylate polymers are the most commonly used leveling agents for powder coatings. However, in actual construction, most polyacrylate leveling agents will still be accompanied by phenomena such as blooming, orange peel, shrinkage craters, and pinholes during the drying process. The occurrence of these phenomena not only affects the appearance of the product, but also reduces the adhesion strength and protective performance of the coating. Summary of the invention

[0004] In order to solve the problems existing in the background technology, the present invention provides a leveling agent for powder coatings and a preparation method and application thereof, which can ensure a high leveling grade while avoiding surface defects of the coating such as blooming, orange peel, craters and pinholes.

[0005] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a method for preparing a leveling agent for powder coatings, comprising the following steps:

[0006] S1. Add 30 parts of acrylate and 0.2-0.5 parts of glycidyl methacrylate into a reaction kettle by weight, stir evenly, heat to 70-80°C, weigh 40-50 parts of deionized water and 0.5-1.5 parts of tert-butyl perbenzoate, and add dropwise into the reaction kettle for 0.5-1.5h. After the addition is complete, react at a constant temperature for 0.5-1.5h.

[0007] S2, add 4-8 parts of modified silica to the reaction kettle, cool to 50-60°C, and stir at high speed for 2-3h to obtain polyacrylate emulsion;

[0008] S3. Add 8-12 parts of epoxy phosphate to the polyacrylate emulsion obtained in S2 under stirring, continue stirring, react for 2-5 hours, cool naturally to room temperature, adjust the pH to 7-8 with ammonia water, filter, and obtain a leveling agent for powder coating.

[0009] Furthermore, in S2, the preparation method of the modified silica is as follows: by weight, 5 parts of nano-silica and 10-20 parts of toluene are weighed, mixed, added to a stirring device, stirred and dispersed for 0.5-1.5 hours, and then 0.2-0.4 parts of a fluorine-containing silane coupling agent are added. The mixture is heated in an oil bath under nitrogen protection to 70-80°C, reacted for 2-3 hours, filtered, washed with toluene, vacuum dried for 2-3 hours, and ground to obtain the modified silica.

[0010] Furthermore, the fluorine-containing silane coupling agent includes heptadecafluorodecyltriethoxysilane or heptadecafluorodecyltrimethoxysilane.

[0011] Further, in S3, the preparation process of the epoxy phosphate is as follows:

[0012] A1. Weigh 20 parts of epoxy resin and 6-9 parts of eleostearic acid by weight, add them into a reactor, mix well, then add 0.3-0.6 parts of N,N-dicyclohexylcarbodiimide, heat to 90°C-110°C, and keep warm for 6-8h;

[0013] A2. The temperature of the reactor is lowered to 60-80°C, and 8-12 parts of a mixture of alcohol ether phosphate and n-butanol in a mass ratio of 1:1 are added dropwise into the reactor for 0.5-1.5 hours. After the addition is completed, the reaction is kept warm for 4-5 hours to obtain epoxy phosphate.

[0014] Furthermore, in S1, the acrylic acid ester includes butyl methacrylate and / or ethyl methacrylate.

[0015] In a second aspect, the present invention provides a leveling agent for powder coatings, which is prepared by the above-mentioned preparation method.

[0016] In a third aspect, the present invention provides an application of a leveling agent for powder coatings, wherein the leveling agent for powder coatings is prepared by the above-mentioned preparation method, and the leveling agent for powder coatings is used to prepare high-leveling powder coatings, which comprises the following raw material components by mass percentage: 15-20% polyester resin, 20-30% filler, 3-5% curing agent, 0.5-1% benzoin, 0.6-1.2% leveling agent, 0.5-2% pigment, 1.2-2.0% chelating agent and remainder epoxy resin.

[0017] Furthermore, the preparation method of the high-leveling powder coating is as follows: all raw material components are put into a mixing tank for premixing to obtain a premix; then the premix is ​​put into a twin-screw extruder for extrusion, tableting, crushing, and screening to obtain a high-leveling powder coating; the particle size of the high-leveling powder coating is 25-80μm.

[0018] Furthermore, the chelating agent is sodium tripolyphosphate.

[0019] Furthermore, the curing agent includes one of diethylenetriamine, diethylaminopropylamine, and meta-phenylenediamine, or a mixture of at least two of them.

[0020] This application has the following beneficial effects:

[0021] 1. The present invention modifies nano silicon dioxide by using a fluorine-containing silane coupling agent, so that fluorine atoms are introduced into the organic molecular chain segments. Since fluorine atoms have the properties of small radius and strong electronegativity, the surface tension of the leveling agent is greatly reduced. In addition, fluorine atoms can easily migrate from the inside to the outside, resulting in a small surface tension, which can improve the compatibility and migration ability of nano silicon dioxide in the resin, so that the leveling agent can be freely dispersed on the surface of the paint film, and the flow rate and anti-shrinkage ability of the coating are improved, thereby improving the leveling effect of the coating; by grafting polyacrylate molecular chain segments on the surface of the modified silicon dioxide, the uniform dispersion in the coating is further achieved; by introducing epoxy phosphate to modify the polyacrylate molecular chain segments, the leveling agent can provide more reaction sites when the powder coating is cured, greatly improving the compatibility of the leveling agent with polyester resin and epoxy resin, increasing the crosslinking density of resin molecules, reducing fine holes, making the coating surface smooth and uniform, and better improving the surface defects of the coating.

[0022] 2. After the powder coating is sprayed on the metal surface, the chelating agent in the coating component can chelate with the surface metal ions to enhance the adhesion of the coating to the metal surface. At the same time, the epoxy phosphate segments, polyacrylate segments and chelating agents can form a three-dimensional network structure through intermolecular bonding, thereby enhancing the internal cross-linking density, improving the wetting ability and bonding performance of the bottom of the coating, and enhancing the adhesion and leveling effect of the coating, thereby improving the adhesion and surface leveling of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The figure is a comparative trend chart of the coating film adhesion and leveling grade of the powder coatings prepared in Examples 1-5 of the present invention and Comparative Examples 1-6. DETAILED DESCRIPTION

[0024] The present application is further described in detail below with reference to the embodiments.

[0025] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.

[0026] Embodiment 1: A high-leveling powder coating comprises the following raw material components by mass percentage: 18% polyester resin, 25% filler, 4% curing agent, 0.7% benzoin, 0.8% leveling agent, 1% pigment, 1.6% chelating agent and the remainder epoxy resin.

[0027] The preparation method of the high-leveling powder coating is as follows: all raw material components are put into a mixing tank for premixing to obtain a premix; then the premix is ​​put into a twin-screw extruder for extrusion, tableting, crushing and screening to obtain the high-leveling powder coating; the particle size of the high-leveling powder coating is 25-80μm.

[0028] The polyester resin is Zhejiang Tiansong 9011F polyester resin, and the epoxy resin is Shenzhen Jitian E-12 epoxy resin.

[0029] The filler is titanium dioxide, the curing agent is diethylenetriamine, the pigment is carbon black, and the chelating agent is sodium tripolyphosphate. Diethylenetriamine was purchased from Jiangsu Haolong Chemical Co., Ltd. Sodium tripolyphosphate was purchased from Hebei Jiuyu Biotechnology Co., Ltd.

[0030] The preparation method of the leveling agent comprises the following steps:

[0031] S1. Add 30 parts of acrylate and 0.3 parts of glycidyl methacrylate into a reaction kettle by weight, stir evenly, heat to 75°C, weigh 45 parts of deionized water and 1 part of tert-butyl perbenzoate, and drop them into the reaction kettle for 1 hour. After the dropwise addition is completed, react at a constant temperature for 1 hour. The acrylate is butyl methacrylate.

[0032] S2. Add 6 parts of modified silica into the reaction kettle, cool to 55° C., and stir at high speed for 2.5 hours to obtain a polyacrylate emulsion.

[0033] S3, under stirring, add 10 parts of epoxy phosphate to the polyacrylate emulsion obtained in S2, continue stirring, react for 3 hours, cool naturally to room temperature, adjust the pH to 8 with ammonia water, filter, and obtain the leveling agent. Epoxy phosphate was purchased from Shenzhen Hemmings New Materials Co., Ltd.

[0034] In S2, the preparation method of modified silicon dioxide is as follows: by weight, 5 parts of nano silicon dioxide and 15 parts of toluene are weighed and mixed, added to a stirring device, stirred and dispersed for 1 hour, and then 0.3 parts of fluorine-containing silane coupling agent are added, heated in an oil bath under nitrogen protection, heated to 75°C, reacted for 2.5 hours, filtered, washed with toluene, vacuum dried for 2.5 hours, and ground to obtain modified silicon dioxide. The fluorine-containing silane coupling agent is heptadecafluorodecyl triethoxysilane, industrial grade, purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.

[0035] In S3, the preparation process of epoxy phosphate is as follows:

[0036] A1. Weigh 20 parts of epoxy resin and 7 parts of eleostearic acid by weight, add them into a reactor, mix well, then add 0.5 parts of N,N-dicyclohexylcarbodiimide, heat to 95°C, and keep the temperature for 7 hours;

[0037] A2. The temperature of the reactor was lowered to 70°C, and 10 parts of a mixture of alcohol ether phosphate and n-butanol in a mass ratio of 1:1 were added dropwise to the reactor for 1 hour. After the addition was completed, the mixture was kept warm for 4.5 hours to obtain epoxy phosphate. Alcohol ether phosphate was purchased from Hai'an Petrochemical Plant in Jiangsu Province, specifically alcohol ether phosphate MOA-9P.

[0038] Example 2: The difference between this example and Example 1 is that the proportions of raw material components of the high-leveling powder coating are different.

[0039] Specifically, a high-leveling powder coating comprises the following raw material components by mass percentage: 15% polyester resin, 20% filler, 3% curing agent, 0.5% benzoin, 0.6% leveling agent, 0.5% pigment, 1.2% chelating agent and the remainder epoxy resin.

[0040] Example 3: The difference between this example and Example 1 is that the proportions of raw material components of the high-leveling powder coating are different.

[0041] Specifically, a high-leveling powder coating comprises the following raw material components by mass percentage: 20% polyester resin, 30% filler, 5% curing agent, 1% benzoin, 1.2% leveling agent, 2% pigment, 2.0% chelating agent and the remainder epoxy resin.

[0042] Example 4: The difference between this example and Example 1 is that the amount of each raw material component used in the preparation of the leveling agent is different.

[0043] Specifically, the preparation method of the leveling agent comprises the following steps:

[0044] S1. Add 30 parts of acrylate and 0.2 parts of glycidyl methacrylate into a reaction kettle by weight, stir evenly, heat to 75°C, weigh 40 parts of deionized water and 0.5 parts of tert-butyl perbenzoate, and drop them into the reaction kettle. The drop time is 1 hour. After the drop addition is completed, react at a constant temperature for 1 hour. The acrylate is butyl methacrylate.

[0045] S2. Add 4 parts of modified silica into the reaction kettle, cool to 55°C, and stir at high speed for 2.5 hours to obtain a polyacrylate emulsion.

[0046] S3. Add 8 parts of epoxy phosphate to the polyacrylate emulsion obtained in S2 under stirring, continue stirring, react for 3 hours, cool naturally to room temperature, adjust the pH to 8 with ammonia water, filter, and obtain the leveling agent.

[0047] Example 5: The difference between this example and Example 1 is that in the preparation of the leveling agent, the amounts of the raw material components are different.

[0048] Specifically, the preparation method of the leveling agent comprises the following steps:

[0049] S1. Add 30 parts of acrylate and 0.5 parts of glycidyl methacrylate into a reaction kettle by weight, stir evenly, heat to 75°C, weigh 50 parts of deionized water and 1.5 parts of tert-butyl perbenzoate, and drop them into the reaction kettle. The drop time is 1 hour. After the drop addition is completed, react at a constant temperature for 1 hour. The acrylate is butyl methacrylate.

[0050] S2. Add 8 parts of modified silica into the reaction kettle, cool to 55° C., and stir at high speed for 2.5 hours to obtain a polyacrylate emulsion.

[0051] S3. Under stirring, add 12 parts of epoxy phosphate to the polyacrylate emulsion obtained in S2, continue stirring, react for 3 hours, cool naturally to room temperature, adjust the pH to 8 with ammonia water, filter, and obtain the leveling agent.

[0052] Comparative Example 1: The difference between this comparative example and Example 1 is that in the preparation of modified silica, the fluorine-containing silane coupling agent is replaced by a fluorine-free silane coupling agent, that is, heptadecafluorodecyltriethoxysilane is replaced by γ-aminopropyltriethoxysilane.

[0053] Comparative Example 2: The difference between this comparative example and Example 1 is that epoxy phosphate is deleted in the preparation of the leveling agent.

[0054] Specifically, the preparation method of the leveling agent comprises the following steps:

[0055] S1. Add 30 parts of acrylate and 0.3 parts of glycidyl methacrylate into a reaction kettle by weight, stir evenly, heat to 75°C, weigh 45 parts of deionized water and 1 part of tert-butyl perbenzoate, and drop them into the reaction kettle for 1 hour. After the dropwise addition is completed, react at a constant temperature for 1 hour. The acrylate is butyl methacrylate.

[0056] S2. Add 6 parts of modified silica into the reaction kettle, cool to 55° C., and stir at high speed for 2.5 hours to obtain a polyacrylate emulsion.

[0057] S3. Cool naturally to room temperature, adjust the pH to 8 with ammonia water, and filter to obtain the leveling agent.

[0058] Comparative Example 3: The difference between this comparative example and Example 1 is that in the preparation of modified silica, the fluorine-containing silane coupling agent is replaced by a fluorine-free silane coupling agent, that is, heptadecafluorodecyltriethoxysilane is replaced by γ-aminopropyltriethoxysilane; and, in the preparation of the leveling agent, epoxy phosphate is deleted.

[0059] Comparative Example 4: The difference between this comparative example and Example 1 is that in the preparation of the high-leveling powder coating, the leveling agent is replaced by a commercially available acrylic leveling agent, model VOK-FLOW-100.

[0060] Comparative Example 5: The difference between this comparative example and Example 1 is that in the preparation of the high-leveling powder coating, the raw material component chelating agent is deleted.

[0061] Specifically, a high-leveling powder coating comprises the following raw material components by mass percentage: 18% polyester resin, 25% filler, 4% curing agent, 0.7% benzoin, 0.8% leveling agent, 1% pigment and the remainder epoxy resin.

[0062] Comparative Example 6: The difference between this comparative example and Example 1 is that in the preparation of the high-leveling powder coating, the leveling agent is replaced by a commercially available acrylic leveling agent, model VOK-FLOW-100; and the raw material component chelating agent is deleted.

[0063] Test example: The high-leveling powder coatings obtained in Examples 1-5 and Comparative Examples 1-5 were sprayed on stainless steel plates respectively by electrostatic spraying. The voltage of the spray gun reached 100kV to ensure maximum coverage. During spraying, the distance between the spray gun and the stainless steel plate was kept at about 140mm to achieve a good atomization effect and avoid the generation of breakdown points. In order to ensure the uniformity of the coating, the speed of the spray gun was kept at about 0.1 m / s. The sprayed stainless steel plate was sent to an oven and baked at 180°C for 10 minutes to solidify into a strong and bright coating with a thickness of about 90um. Then, the performance of each coating was tested.

[0064] Test items and basis: 1. Adhesion (normal temperature) - GB / T9286-2014, Level 0 is the best, Level 1 is the second best, the larger the number, the worse the adhesion.

[0065] 2. Leveling grade - refer to GB / T 1728-2020, and then compare with the special leveling standard comparison plate for powder coating. There are 10 standard comparison plates, and the corresponding leveling grades are 1-10, among which grade 1 is the worst and grade 10 is the best.

[0066] 3. Appearance evaluation - Observe the appearance of the coating with the naked eye to check whether there are problems such as blooming, orange peel, craters and pinholes.

[0067] Test results: See Table 1.

[0068] Table 1. Test results of the experimental example

[0069] Adhesion / Grade Leveling grade / level Appearance evaluation Example 1 0 8 No blooming, orange peel, shrinkage holes or pinholes Example 2 0 8 No blooming, orange peel, shrinkage holes or pinholes Example 3 1 8 No blooming, orange peel, shrinkage holes or pinholes Example 4 1 8 No blooming, orange peel, shrinkage holes or pinholes Example 5 0 8 No blooming, orange peel, shrinkage holes or pinholes Comparative Example 1 1 6 No blooming, no orange peel, a small amount of shrinkage holes and pinholes Comparative Example 2 2 6 No blooming, no orange peel, a small amount of shrinkage holes and pinholes Comparative Example 3 3 5 No blooming, no orange peel, but with many shrinkage holes and pinholes Comparative Example 4 3 5 Localized flowery and orange peel, with a small amount of shrinkage holes and pinholes Comparative Example 5 2 6 Local blooming and orange peel, no shrinkage holes and pinholes Comparative Example 6 3 5 Localized flowery and orange peel, with a small amount of shrinkage holes and pinholes

[0070] Result analysis:

[0071] Analyze Examples 1-5 and combine the data in Table 1 and Figure 1 It can be seen that the high-leveling powder coating prepared by the present invention has excellent coating film adhesion (lower than grade 1), excellent leveling grade (up to grade 8) when used, and no flowery and orange peel, shrinkage cavities and pinhole defects in appearance.

[0072] Analyze Example 1 and Comparative Example 1 and combine the data in Table 1 and Figure 1 It can be seen that when the fluorine-containing silane coupling agent is replaced by a fluorine-free silane coupling agent, the leveling grade drops to level 6, and there are a small number of craters and pinholes on the appearance of the coating film. This shows that in the preparation of the leveling agent, the fluorine-containing silane coupling agent is used to modify the nano-silica, that is, the introduction of fluorine is beneficial to improve the leveling grade of the final powder coating, which is beneficial to improve the appearance of the coating film and avoid the appearance of craters and pinholes.

[0073] Analyze Example 1 and Comparative Example 2 and combine the data in Table 1 and Figure 1 It can be seen that in the preparation of the leveling agent, if epoxy phosphate is deleted, the adhesion of the coating film will deteriorate from grade 0 to grade 2, and the leveling grade will deteriorate from grade 8 to grade 6. In addition, there are a small number of shrinkage holes and pinholes on the appearance of the coating film, indicating that the introduction of epoxy phosphate chain segments can improve the adhesion of the coating film, improve the leveling grade, and reduce the fine holes in the coating film, making the coating surface smooth, uniform and defect-free.

[0074] Analyze Example 1 and Comparative Examples 1-3 and combine the data in Table 1 and Figure 1 It can be seen that the introduction of fluorine and epoxy phosphate segments can synergistically improve the adhesion of the coating, improve the leveling grade and avoid appearance defects.

[0075] Analyze Example 1 and Comparative Examples 4-6 and combine the data in Table 1 and Figure 1 It can be seen that the use effect of the commercially available leveling agent (VOK-FLOW-100 type acrylate leveling agent) in powder coatings is worse than that of the leveling agent prepared by the present invention in all aspects (coating film adhesion, leveling grade and appearance performance). Deleting the raw material component chelating agent in the high-leveling powder coating of the present invention alone will also cause the coating film of the high-leveling powder coating to deteriorate in all aspects (coating film adhesion, leveling grade and appearance performance). In addition, analysis shows that there is a synergistic effect between the chelating agent and the leveling agent prepared by the present invention, but there is no synergistic effect between the chelating agent and the commercially available leveling agent (VOK-FLOW-100 type acrylate leveling agent).

[0076] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0077] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a leveling agent for powder coating, characterized in that: The steps include: S1. Add 30 parts of acrylate and 0.2-0.5 parts of glycidyl methacrylate into a reaction kettle by weight, stir evenly, heat to 70-80°C, weigh 40-50 parts of deionized water and 0.5-1.5 parts of tert-butyl perbenzoate, and add dropwise into the reaction kettle for 0.5-1.5h. After the addition is complete, react at a constant temperature for 0.5-1.5h. S2, add 4-8 parts of modified silica to the reaction kettle, cool to 50-60°C, and stir at high speed for 2-3h to obtain polyacrylate emulsion; S3. Add 8-12 parts of epoxy phosphate to the polyacrylate emulsion obtained in S2 under stirring, continue stirring, react for 2-5 hours, cool naturally to room temperature, adjust the pH to 7-8 with ammonia water, filter, and obtain a leveling agent for powder coating.

2. The method for preparing a leveling agent for powder coating according to claim 1, characterized in that: In S2, the preparation method of the modified silica is as follows: weigh 5 parts of nano-silica and 10-20 parts of toluene by weight, add them to a stirring device, stir and disperse for 0.5-1.5 hours, add 0.2-0.4 parts of fluorine-containing silane coupling agent, heat in an oil bath under nitrogen protection, raise the temperature to 70-80°C, react for 2-3 hours, filter, wash with toluene, vacuum dry for 2-3 hours, and grind to obtain modified silica.

3. The method for preparing a leveling agent for powder coating according to claim 2, characterized in that: The fluorine-containing silane coupling agent includes heptadecafluorodecyltriethoxysilane or heptadecafluorodecyltrimethoxysilane.

4. The method for preparing a leveling agent for powder coating according to claim 1, characterized in that: In S3, the preparation process of the epoxy phosphate is as follows: A1. Weigh 20 parts of epoxy resin and 6-9 parts of eleostearic acid by weight, add them into a reactor, mix well, then add 0.3-0.6 parts of N,N-dicyclohexylcarbodiimide, heat to 90°C-110°C, and keep warm for 6-8h; A2. The temperature of the reactor is lowered to 60-80°C, and 8-12 parts of a mixture of alcohol ether phosphate and n-butanol in a mass ratio of 1:1 are added dropwise into the reactor for 0.5-1.5 hours. After the addition is completed, the reaction is kept warm for 4-5 hours to obtain epoxy phosphate.

5. The method for preparing a leveling agent for powder coating according to claim 1, characterized in that: In S1, the acrylic acid ester includes butyl methacrylate and / or ethyl methacrylate.

6. A leveling agent for powder coating, characterized in that: The method is prepared according to any one of claims 1 to 5.

7. Application of a leveling agent for powder coating, characterized in that: The leveling agent for powder coating is prepared by the preparation method according to any one of claims 1 to 5. The leveling agent for powder coating is used to prepare high-leveling powder coating, and comprises the following raw material components by mass percentage: 15-20% polyester resin, 20-30% filler, 3-5% curing agent, 0.5-1% benzoin, 0.6-1.2% leveling agent, 0.5-2% pigment, 1.2-2.0% chelating agent and the remainder epoxy resin.

8. The use of the leveling agent for powder coating according to claim 7, characterized in that: The preparation method of the high-leveling powder coating is as follows: all raw material components are put into a mixing tank for premixing to obtain a premix; then the premix is ​​put into a twin-screw extruder for extrusion, tableting, crushing and screening to obtain a high-leveling powder coating; the particle size of the high-leveling powder coating is 25-80 μm.

9. The use of the leveling agent for powder coating according to claim 7, characterized in that: The chelating agent is sodium tripolyphosphate.

10. The use of the leveling agent for powder coating according to claim 7, characterized in that: The curing agent includes one of diethylenetriamine, diethylaminopropylamine and metaphenylenediamine or a mixture of at least two of them.