Main chain charged fused heterocycle polyelectrolyte and preparation method and application thereof
By introducing a main-chain charged fused heterocyclic structure into the polyelectrolyte and using a rhodium-catalyzed reaction to prepare it in one step, the problem in the existing technology that the charge is mainly in the side chain is solved, and the direct control of the fluorescence properties and the improvement of the aggregated state luminescence properties are achieved. Improved, it has unique application value in the fields of optical devices and protein detection.
Patent Information
- Application Number
- CN202410927596.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The charges in existing polyelectrolytes are mainly bound to the side chains of conjugated polymers, making it difficult to directly affect the electronic properties of the conjugated main chain, limiting the adjustment of photophysical properties.
Provides a main chain charged condensed heterocyclic polyelectrolyte, which is prepared in one step through a rhodium-catalyzed C-H activation cyclization reaction. The condensed heterocyclic charged groups in the main chain are used to control the fluorescence properties, and has high yield and good solubility and thermal properties. stability.
It achieves convenient control of fluorescence properties, enhances aggregated state luminescence performance, and has unique application value in the fields of optical devices and protein detection.
Smart Images

Figure CN118725265A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer technology, and in particular to a main chain charged fused heterocyclic polyelectrolyte and a preparation method and application thereof. Background Art
[0002] Polyelectrolytes are an important class of functional polymer materials, in which the repeating units contain ionizable groups. The fluorescence properties can be conveniently regulated by leveraging the electron push / pull capability of the charged aromatic groups, while giving the products special properties such as photosensitivity, reactive oxygen generation capability, and acid-base responsiveness.
[0003] In existing polyelectrolytes, the charges are mostly bound to the side chains of conjugated polymers. However, it is difficult for side chain polyelectrolytes to directly affect the electronic properties of the conjugated main chain, and they have certain limitations in regulating photophysical properties.
[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0005] Based on the above-mentioned deficiencies of the prior art, the purpose of the present invention is to provide a main chain charged fused heterocyclic polyelectrolyte and its preparation method and application, aiming to solve the problem that the charges of the existing polyelectrolytes are mostly bound to the side chains of conjugated polymers.
[0006] The technical solution of the present invention is as follows:
[0007] In a first aspect of the present invention, a main chain charged fused heterocyclic polyelectrolyte is provided, wherein the main chain charged fused heterocyclic polyelectrolyte has the general structural formula:
[0008]
[0009] wherein x, y, z, and w are each independently an integer between 1 and 200 (specifically, 1, 2, 5, 10, 15, 20, 50, 70, 80, 100, 120, 130, 150, 180 or 200, etc.);
[0010] R 1 is an aryl group, an aryl derivative, an unsubstituted alkyl group (such as methyl, ethyl, propyl, butyl, etc., but not limited thereto) or a substituted alkyl group (such as alkoxy, etc., but not limited thereto);
[0011] R 2 The alkyl group may be an aryl group, an aryl derivative, a nitro group, a cyano group, an unsubstituted alkyl group (such as a methyl group, an ethyl group, a propyl group, a butyl group, etc., but not limited thereto), a substituted alkyl group (such as a trifluoromethyl group; an alkoxy group, specifically a methoxy group, etc.; an alkyl group containing an ester group, such as an alkyl ester group, specifically a CH 3 COO-, etc.; alkyl groups containing ketocarbonyl groups such as alkane copper carbonyl groups, such as CH3 CO-, etc.; of course not limited thereto), sulfur atoms, selenium atoms, hydrogen atoms, halogen atoms (such as F, Cl, Br or I, etc.) or biologically active fragments, wherein the biologically active fragments include one of terpenes, steroids, fatty alcohols and vitamins;
[0012] is an aryl group or an aryl derivative;
[0013] Selected from (Right now ), (Right now ), One of them.
[0014] The polyelectrolyte provided by the present invention is a polycyclic fused main chain charged polyelectrolyte, i.e., a main chain charged fused heterocyclic polyelectrolyte, which has special aggregated luminescent properties, good solubility (soluble in dichloromethane, methanol, acetonitrile, N,N-dimethylformamide, and dimethyl sulfoxide), film-forming property, excellent thermal stability and morphological stability, and has unique potential application value in the fields of optical devices, protein detection, etc. The main chain charged fused heterocyclic polyelectrolyte provided by the present invention effectively solves the problem that the charges of the existing polyelectrolytes are mostly combined on the side chains of the conjugated polymers and are difficult to directly affect the electronic properties of the conjugated main chain, and have certain limitations in the regulation of photophysical properties.
[0015] The main chain charged fused heterocyclic polyelectrolyte provided by the present invention can not only continue the excellent properties of traditional side chain conjugated polyelectrolytes, but also utilize the strong push / pull electron ability of the fused heterocyclic charged groups in the main chain to directly and conveniently regulate the electronic properties such as absorption and emission of the fluorescent polyelectrolyte, thus providing great convenience for the regulation of its physical and chemical properties.
[0016] Aggregation-induced emission is an effect in which molecules do not emit light or emit light weakly in the solution state, but emit light more strongly in the aggregated state. The current mainstream explanation for the principle of aggregation-induced emission is the mechanism of restricted intramolecular motion: in solution, the twisted structure of the excited state of the molecule changes greatly, which makes the reorganization energy of the twist vibration very large, providing an efficient energy dissipation channel for the non-radiative transition process. In the aggregated state, the "confined" environment formed by the intermolecular interaction greatly limits the change of the molecular twisted structure, making the reorganization energy of the twist vibration smaller, effectively blocking the non-radiative transition channel, and the radiative transition process dominates, and the molecule exhibits strong fluorescence. There are a large number of freely rotatable rotor side groups in the main chain charged fused heterocyclic polyelectrolyte repeating unit provided by the present invention. In the solution state, the rotor rotates freely, which is mainly manifested as non-radiative transition. In the aggregated state, due to the π-π stacking effect, the rotor rotation is restricted, which is manifested as radiative transition, and the luminescence effect is enhanced. Therefore, the main chain charged fused heterocyclic polyelectrolyte provided by the present invention exhibits aggregated luminescence performance based on the mechanism of restricted intramolecular motion.
[0017] when for When the main chain charged fused heterocyclic polyelectrolyte is of the general structural formula:
[0018]
[0019] Optionally, R 1 Selected from one of the following structural formulas 1 to 25:
[0020]
[0021]
[0022] in, represents a connection point; m, p, q, and r are each independently an integer between 1 and 20 (for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20, etc.); R and R' are each independently a hydrogen atom, a halogen atom (for example, F, Cl, Br, or I, etc.), a sulfur atom, a selenium atom, a nitro group, a cyano group, an unsubstituted alkyl group (for example, a methyl group, an ethyl group, a propyl group, a butyl group, etc., but of course not limited thereto), a substituted alkyl group (for example, a trifluoromethyl group; an alkoxy group, specifically a methoxy group, etc.; an alkyl group containing an ester group, such as an alkyl ester group, specifically a CH 3 COO-, etc.; alkyl groups containing ketocarbonyl groups such as alkane copper carbonyl groups, such as CH 3CO-, etc.; of course not limited thereto), aryl, aryl derivatives (such as heteroaryl, etc., specifically such as pyridine group, thiophene group, furan group, indole group, etc., of course not limited thereto) or biologically active fragments, wherein the biologically active fragments include one of terpenes, steroids, fatty alcohols and vitamins;
[0023] X is one of an oxygen atom, a sulfur atom and a selenium atom.
[0024] Optionally, R 2 Selected from one of the following structural formulas 26 to 35:
[0025]
[0026] in, Indicates a connection;
[0027] s and t are each independently an integer between 0 and 20 (for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, etc.);
[0028] R and R' are each independently a hydrogen atom, a halogen atom (such as F, Cl, Br or I), a sulfur atom, a selenium atom, a nitro group, a cyano group, an unsubstituted alkyl group (such as methyl, ethyl, propyl, butyl, etc., but not limited thereto), a substituted alkyl group (such as trifluoromethyl; an alkoxy group, specifically a methoxy group, etc.; an alkyl group containing an ester group, such as an alkyl ester group, specifically a CH 3 COO-, etc.; alkyl groups containing ketocarbonyl groups such as alkane copper carbonyl groups, such as CH 3 CO-, etc.; of course not limited thereto), aryl, aryl derivatives (such as heteroaryl, etc., specifically pyridine group, thiophene group, furan group, indole group, etc.) or biologically active fragments, wherein the biologically active fragments include one of terpenes, steroids, fatty alcohols and vitamins.
[0029] Optionally, Select one of the following structural formulas:
[0030]
[0031] Indicates a connection.
[0032] The second aspect of the present invention provides a method for preparing the main chain charged fused heterocyclic polyelectrolyte as described above, which comprises the following steps:
[0033] Adding a bipyridine-substituted aromatic compound, an internal alkyne monomer, a rhodium catalyst and an additive into a solvent, and reacting to obtain the main chain charged fused heterocyclic polyelectrolyte;
[0034] The structural formula of the bipyridine substituted aromatic compound is:
[0035] The structural formula of the internal alkyne monomer is:
[0036] R 1 The alkyl group is an aryl group, an aryl derivative, an unsubstituted alkyl group (such as methyl, ethyl, propyl, butyl, etc., but not limited thereto) or a substituted alkyl group (such as trifluoromethyl; an alkoxy group, specifically a methoxy group, etc.; an alkyl group containing an ester group, such as an alkyl ester group, specifically a CH 3 COO-, etc.; alkyl groups containing ketocarbonyl groups such as alkane copper carbonyl groups, such as CH 3 CO-etc.; of course not limited to this);
[0037] R 2 The alkyl group may be an aryl group, an aryl derivative, a nitro group, a cyano group, an unsubstituted alkyl group (such as a methyl group, an ethyl group, a propyl group, a butyl group, etc., but not limited thereto), a substituted alkyl group (such as a trifluoromethyl group; an alkoxy group, specifically a methoxy group, etc.; an alkyl group containing an ester group, such as an alkyl ester group, specifically a CH 3 COO-, etc.; alkyl groups containing ketocarbonyl groups such as alkane copper carbonyl groups, such as CH 3 CO-, etc.; of course not limited thereto), sulfur atoms, selenium atoms, hydrogen atoms, halogen atoms (such as F, Cl, Br or I, etc.) or biologically active fragments, wherein the biologically active fragments include one of terpenes, steroids, fatty alcohols and vitamins;
[0038] is an aryl group or an aryl derivative;
[0039] The additive includes one of silver trifluoroacetate, silver trifluoromethanesulfonate, silver p-toluenesulfonate and anhydrous copper acetate.
[0040] At present, the types of main chain charged fluorescent polyelectrolyte structures are rare, and there are still few reports on the synthesis method that can efficiently prepare the main chain charged conjugated polyelectrolyte in one step through cheap and easily available monomer raw materials. The difficulty in synthesizing conjugated polyelectrolytes greatly limits the diversity of the structure and function of fluorescent polyelectrolytes. Therefore, it is of great significance to develop a convenient, economical and efficient new polymerization reaction to achieve the efficient construction of a main chain charged fluorescent polyelectrolyte with a novel structure. Based on this, the present invention provides a preparation method as described above, which is simple and efficient, and only requires a one-step reaction, i.e., a rhodium-catalyzed CH activation cyclization reaction, to obtain the target product, and has a high yield (yield of up to 98.0%), and the raw materials used are cheap and easily available. The prepared main chain charged fused heterocyclic polyelectrolyte has a high molecular weight (weight average molecular weight up to 231000, polymer dispersity index of 1.29-1.69), has a special aggregated luminescence performance, and has unique potential application value in the fields of optical devices and protein detection.
[0041] Optionally, the rhodium catalyst includes dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer; and the solvent includes at least one of acetonitrile, methanol, 1,2-dichloroethane, N,N-dimethylformamide and dimethyl sulfoxide, but is not limited thereto.
[0042] Optionally, the molar ratio of the internal acetylene monomer, the bipyridine-substituted aromatic compound, the rhodium catalyst and the additive is 1:(0.5-1.25):(0.1-0.5):(2.3-9.5); for example, the molar ratio of the internal acetylene monomer, the bipyridine-substituted aromatic compound, the rhodium catalyst and the additive is 1:0.5:0.1:2.3, 1:1.25:0.5:9.2, 1:1:0.25:6, 1:0.5:0.1:9 or 1:0.75:0.3:7, etc.
[0043] The reaction concentration of the internal acetylenic monomer is 0.05 to 2 mol / L (for example, 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.5 mol / L, 1 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L or 2 mol / L, etc.);
[0044] The reaction conditions are:
[0045] inert gas atmosphere, the reaction temperature is 100-140°C (for example, 100°C, 110°C, 120°C, 130°C or 140°C), and the reaction time is 12-24h (for example, 12h, 15h, 18h, 20h, 22h or 24h, etc.).
[0046] Optionally, after the reaction, before obtaining the main chain charged fused heterocyclic polyelectrolyte, the following steps are further included:
[0047] The reaction solution obtained after the reaction is cooled to room temperature, and filtered to obtain a filtrate;
[0048] The filtrate is added to a precipitant for precipitation, and then filtered and dried.
[0049] The polymer product obtained in the present invention is easy to separate, and only needs to be precipitated once in a precipitant to obtain a main chain charged fused heterocyclic polyelectrolyte with high purity.
[0050] In the present invention, specifically, the reaction solution obtained after the reaction is cooled to room temperature, then diluted with methanol and dichloromethane (the volume ratio of the two can be 1:3), and then simply filtered through neutral alumina to obtain a filtrate; the obtained filtrate is added to a precipitant for precipitation, filtered, and the precipitate is collected and dried to constant weight to obtain the main chain charged fused heterocyclic polyelectrolyte.
[0051] Optionally, the precipitant includes at least one of methanol, ether, acetone and n-hexane, but is not limited thereto;
[0052] The R 1 Selected from one of the following structural formulas 1 to 25, wherein R 2 Selected from one of the following structural formulas 26 to 35, Selected from one of the following structural formulas 36 to 46:
[0053]
[0054]
[0055]
[0056] in, represents a connection; m, p, q, and r are each independently an integer between 1 and 20 (for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, etc.); s and t are each independently an integer between 0 and 20 (for example, 0,
[0057] 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, etc.); R, R' are each independently a hydrogen atom, a halogen atom (such as F, Cl, Br or I, etc.), a nitro group, a cyano group, an unsubstituted alkyl group (such as methyl, ethyl, propyl, etc., but of course not limited thereto), a substituted alkyl group (such as trifluoromethyl; an alkoxy group, specifically a methoxy group, etc.; an alkyl group containing an ester group, such as an alkyl ester group, specifically a CH 3 COO-, etc.; alkyl groups containing ketocarbonyl groups such as alkane copper carbonyl groups, such as CH 3 CO-, etc.; of course not limited to these)), sulfur atoms, selenium atoms, aromatic groups, aromatic group derivatives (such as heteroaromatic groups, etc.) or biologically active fragments, wherein the biologically active fragments include one of terpenes, steroids, fatty alcohols and vitamins.
[0058] The third aspect of the present invention provides an application of the main chain charged fused heterocyclic polyelectrolyte as described above and / or the main chain charged fused heterocyclic polyelectrolyte prepared by the preparation method as described above in the field of optical devices or protein detection.
[0059] Beneficial effects: The polyelectrolyte provided by the present invention is a polycyclic fused main chain charged polyelectrolyte, which has special aggregated luminescence properties, good solubility (such as being soluble in dichloromethane, methanol, acetonitrile, N,N-dimethylformamide, and dimethyl sulfoxide), film-forming properties, excellent thermal stability and morphological stability, and has unique potential application value in the fields of optical devices and protein detection. In addition, the preparation method provided by the present invention is simple and efficient, and only one-step reaction, namely, rhodium-catalyzed CH activation cyclization reaction, is required to obtain the target product, and the yield is high (the yield is as high as 98.0%), and the raw materials used are cheap and easily available. The present invention effectively solves the problem that the charges of existing polyelectrolytes are mostly bound to the side chains of conjugated polymers. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the polyelectrolyte P1 prepared in Example 1 in deuterated dimethyl sulfoxide.
[0061] Figure 2 (A) is a photoluminescence curve of the polyelectrolyte P1 prepared in Example 1 in a dimethyl sulfoxide solution with the same water content, and (B) is a fluorescence emission intensity change trend diagram of the polyelectrolyte P1 prepared in Example 1 in a dimethyl sulfoxide solution with the same water content.
[0062] Figure 3 This is the hydrogen nuclear magnetic resonance spectrum of the polyelectrolyte P2 prepared in Example 2 in deuterated dimethyl sulfoxide.
[0063] Figure 4 (A) is a photoluminescence curve of the polyelectrolyte P2 prepared in Example 2 in a dimethyl sulfoxide solution with the same water content, and (B) is a fluorescence emission intensity change trend diagram of the polyelectrolyte P2 prepared in Example 2 in a dimethyl sulfoxide solution with the same water content.
[0064] Figure 5 (A) is a fluorescence intensity change curve of the polyelectrolyte P2 prepared in Example 2 in PBS solutions with different contents of bovine serum albumin added, and (B) is a fluorescence emission intensity change trend diagram of the polyelectrolyte P2 prepared in Example 2 in PBS solutions with different contents of bovine serum albumin added.
[0065] Figure 6 This is the hydrogen nuclear magnetic resonance spectrum of the polyelectrolyte P3 prepared in Example 3 in deuterated dimethyl sulfoxide.
[0066] Figure 7 This is the hydrogen nuclear magnetic resonance spectrum of the polyelectrolyte P4 prepared in Example 4 in deuterated dimethyl sulfoxide.
[0067] Figure 8 This is the hydrogen nuclear magnetic resonance spectrum of the polyelectrolyte P5 prepared in Example 5 in deuterated dimethyl sulfoxide.
[0068] Fig. 9 (A) is a photoluminescence curve of the polyelectrolyte P5 prepared in Example 5 in dimethyl sulfoxide solutions with different water contents. (B) is a trend diagram of the fluorescence emission intensity of the polyelectrolyte P5 prepared in Example 5 in dimethyl sulfoxide solutions with the same water content. DETAILED DESCRIPTION
[0069] The present invention provides a polyelectrolyte and a preparation method and application thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0070] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0071] The present invention will be further described below by means of specific examples.
[0072] Unless otherwise specified, the raw materials used in the following examples are all commercially available products.
[0073] In the following examples, 1,5-di(2-pyridyl)naphthalene was prepared according to the method disclosed in the literature (Xu K, Fu Y, Zhou Y, et al. Angewandte Chemie, 2017, 129 (50), 16092-16097.), and 4,4'-(1,4-hexenedioxy)bis(phenylacetylene) was prepared according to the method disclosed in the literature (Gao, M.; Lam, JWY; Liu, Y.; Li, J.; Tang, BZ Polymer Chemistry 2013, 4 (9), 2841-2849.).
[0074] 1,6-bis(4-(hex-1-yn-1-yl)phenoxy)hexane was prepared according to the method disclosed in the literature (Gao, M.; Lam, JWY; Liu, Y.; Li, J.; Tang, BZ Polymer Chemistry 2013, 4(9), 2841-2849).
[0075] 1,6-Di(2-pyridyl)pyrene was prepared according to the method disclosed in the literature (Xu K, Fu Y, Zhou Y, et al. Angewandte Chemie, 2017, 129(50), 16092-16097.).
[0076] 1,1′-[1,2-bis[4-(2-phenylethynyl)phenyl]-1,2-vinyl]bibenzene was prepared according to the method disclosed in the literature (Gao, M.; Lam, JWY; Liu, Y.; Li, J.; Tang, BZ Polymer Chemistry 2013, 4(9), 2841-2849).
[0077] Example 1
[0078] This embodiment provides a main chain charged fused heterocyclic polyelectrolyte (referred to as polyelectrolyte P1) and a preparation method thereof. The structural formula of polyelectrolyte P1 is as follows:
[0079]
[0080] The synthetic route of polyelectrolyte P1 is as follows:
[0081]
[0082] The preparation method of polyelectrolyte P1 comprises the following steps:
[0083] (1) Under the protection of inert gas, 47.02 mg of 4,4'-(1,4-hexenedioxy)bis(diphenylacetylene), 28.22 mg of 1,5-di(2-pyridyl)naphthalene, and 18.5 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer ([Cp*RhCl 2 ] 2 ) and 203.21 mg silver trifluoroacetate (AgCF 3 CO 2), added into 1 mL of dry acetonitrile solution to dissolve, stirred for reaction at 120° C. for 12 h; after the reaction was complete, the reaction mother liquor was diluted with 4 mL of dichloromethane and 1 mL of methanol, filtered through a 4 cm high neutral alumina column (200 mesh), and then directly precipitated in 100 mL of ether solution, the precipitate was collected, and vacuum dried at 65° C. to constant weight to obtain polyelectrolyte P1 with a yield of 98.0%, an absolute weight average molecular weight of 231700 g / mol, and a polymer dispersibility index (PDI) of 1.60.
[0084] The H NMR spectrum of the polyelectrolyte P1 prepared in Example 1 in deuterated dimethyl sulfoxide is shown in Figure 1 As shown. Figure 1 It can be seen that the solvent peak and water peak of deuterated dimethyl sulfoxide are located at 2.50ppm and 3.30ppm respectively. In addition, all other signals are hydrogen atom signals of polyelectrolyte P1, and several characteristic hydrogen atom signals can also be assigned accordingly. Among them, 4.0ppm is the characteristic peak of hydrogen atoms on the methylene connected to oxygen on the alkyl chain.
[0085] The photoluminescence curves of the polyelectrolyte P1 prepared in Example 1 in dimethyl sulfoxide solutions with different water contents (i.e., mixed solutions of dimethyl sulfoxide and water with different water contents, the same below, wherein the volume content of water is 0%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80% and 90%, respectively) are shown in FIG. Figure 2 As shown in (A), the fluorescence emission intensity variation trend in dimethyl sulfoxide solutions with different water contents is shown in Figure 2 As shown in (B), I is the fluorescence intensity of polyelectrolyte P1 in dimethyl sulfoxide solutions with different water contents, I 0 is the fluorescence intensity of polyelectrolyte P1 in pure dimethyl sulfoxide solution. Figure 2 As can be seen in (B), with the increase of water content, the fluorescence of polyelectrolyte P1 gradually increases and reaches the maximum at 90% water content. Polyelectrolyte P1 shows obvious aggregation-induced emission phenomenon.
[0086] Example 2
[0087] This embodiment provides a main chain charged fused heterocyclic polyelectrolyte (referred to as polyelectrolyte P2) and a preparation method thereof. The structural formula of polyelectrolyte P2 is as follows:
[0088]
[0089] The synthetic route of polyelectrolyte P2 is as follows:
[0090]
[0091] The preparation method of polyelectrolyte P2 comprises the following steps:
[0092] Under the protection of inert gas, 43.1 mg of 1,6-bis(4-(hex-1-yn-1-yl)phenoxy)hexane, 28.22 mg of 1,5-di(2-pyridyl)naphthalene, 18.5 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer and 203.21 mg of silver trifluoroacetate were added to 1 mL of dry acetonitrile solution for dissolution, and stirred for reaction at 120° C. for 12 h. After the reaction was complete, the reaction mother liquor was diluted with 4 mL of dichloromethane and 1 mL of methanol, filtered through a 4 cm high neutral alumina column (200 mesh), and then directly precipitated in 100 mL of ether solution. The precipitate was collected and dried in vacuum at 65° C. to constant weight to obtain polyelectrolyte P2 with a yield of 91.0%.
[0093] The H NMR spectrum of the polyelectrolyte P2 prepared in Example 2 in deuterated dimethyl sulfoxide is shown in Figure 3 As shown. Figure 3 It can be seen that the solvent peak and water peak of deuterated dimethyl sulfoxide are located at 2.50ppm and 3.30ppm respectively. In addition, all other signals are hydrogen atom signals of polyelectrolyte P2, and several characteristic hydrogen atom signals can also be assigned accordingly. Among them, 4.0ppm is the characteristic peak of hydrogen atoms on the methylene connected to oxygen on the alkyl chain.
[0094] The photoluminescence curves of the polyelectrolyte P2 prepared in Example 2 in dimethyl sulfoxide solutions with different water contents are shown in FIG. Figure 4 As shown in (A), the fluorescence emission intensity variation trend of polyelectrolyte P2 in dimethyl sulfoxide solutions with different water contents is shown in Figure 4 As shown in (B), I is the fluorescence intensity of polyelectrolyte P2 in dimethyl sulfoxide solutions with different water contents, I 0 is the fluorescence intensity of polyelectrolyte P2 in pure dimethyl sulfoxide solution. Figure 4 As can be seen in (B), with the increase of water content, the fluorescence of polyelectrolyte P2 gradually increases and reaches the maximum at 90% water content. Polyelectrolyte P2 exhibits obvious aggregation-induced emission phenomenon.
[0095] The protein detection application results of the polyelectrolyte P2 prepared in Example 2 are as follows Figure 5 As shown, I is the fluorescence intensity of polyelectrolyte P2 in PBS buffer with different bovine serum albumin contents, I 0 is the fluorescence intensity of polyelectrolyte P2 in pure PBS buffer. Figure 5In the experiment, polyelectrolyte P2 interacted with different amounts of bovine serum albumin (BSA) (0 μl, 5 μl, 15 μl, 25 μl, 45 μl, 65 μl, 100 μl, 150 μl, 200 μl, 250 μl, 300 μl and 400 μl) in PBS buffer (3 mL), causing the fluorescence intensity of polyelectrolyte P2 to change. As the content of BSA increased, the fluorescence intensity of polyelectrolyte P2 in the solution first weakened and then increased. This indicates that the polyelectrolyte provided by the present invention can be used in the field of protein detection technology.
[0096] Example 3
[0097] This embodiment provides a main chain charged fused heterocyclic polyelectrolyte (referred to as polyelectrolyte P3) and a preparation method thereof. The structural formula of polyelectrolyte P3 is as follows:
[0098]
[0099] The synthetic route of polyelectrolyte P3 is as follows:
[0100]
[0101] The preparation method of polyelectrolyte P3 comprises the following steps:
[0102] Under the protection of inert gas, 47.02 mg of 4,4'-(1,4-hexenedioxy)bis(diphenylacetylene), 33.2 mg of 1,5-di(2-pyridyl)anthracene, 18.5 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer and 203.21 mg of silver trifluoroacetate were added to 1 mL of dry acetonitrile solution for dissolution, and stirred for reaction at 120°C for 12 h. After the reaction was complete, the reaction mother liquor was diluted with 4 mL of dichloromethane and 1 mL of methanol, filtered through a 4 cm high neutral alumina column (200 mesh), and then directly precipitated in 100 mL of ether solution. The precipitate was collected and dried in vacuum at 65°C to constant weight to obtain polyelectrolyte P3 with a yield of 86.2%.
[0103] The H NMR spectrum of the polyelectrolyte P3 prepared in Example 3 in deuterated dimethyl sulfoxide is shown in Figure 6 As shown. Figure 6 It can be seen that the solvent peak and water peak of deuterated dimethyl sulfoxide are located at 2.50ppm and 3.30ppm respectively, and the solvent peak of residual dichloromethane is at 5.76ppm. In addition, all other signals are hydrogen atom signals of polyelectrolyte P3, and several characteristic hydrogen atom signals can also be assigned accordingly. Among them, the peak at 4.0ppm is the characteristic peak of hydrogen atoms on the methylene connected to oxygen on the alkyl chain.
[0104] Example 4
[0105] This embodiment provides a main chain charged fused heterocyclic polyelectrolyte (referred to as polyelectrolyte P4) and a preparation method thereof. The structural formula of polyelectrolyte P4 is as follows:
[0106]
[0107] The synthetic route of polyelectrolyte P4 is as follows:
[0108]
[0109] The preparation method of polyelectrolyte P4 comprises the following steps:
[0110] Under the protection of inert gas, 47.02 mg of 4,4'-(1,4-hexenedioxy)bis(diphenylacetylene), 35.6 mg of 1,6-di(2-pyridyl)pyrene, 18.5 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer and 203.21 mg of silver trifluoroacetate were added to 1 mL of dry acetonitrile solution for dissolution, and stirred for reaction at 12°C for 12 h. After the reaction was complete, the reaction mother liquor was diluted with 4 mL of dichloromethane and 1 mL of methanol, filtered through a 4 cm high neutral alumina column (200 mesh), and then directly precipitated in 100 mL of ether solution. The precipitate was collected and dried in vacuum at 65°C to constant weight to obtain polyelectrolyte P4 with a yield of 91.1%.
[0111] The H NMR spectrum of the polyelectrolyte P4 prepared in Example 4 in deuterated dimethyl sulfoxide is shown in Figure 7 As shown. Figure 7 It can be seen that the solvent peak and water peak of deuterated dimethyl sulfoxide are located at 2.50ppm and 3.30ppm respectively, and the solvent peak of residual dichloromethane is at 5.76ppm. In addition, all other signals are hydrogen atom signals of polyelectrolyte P4, and several characteristic hydrogen atom signals can also be assigned accordingly. Among them, the peak at 4.0ppm is the characteristic peak of hydrogen atoms on the methylene connected to oxygen on the alkyl chain.
[0112] Example 5
[0113] This embodiment provides a main chain charged fused heterocyclic polyelectrolyte (referred to as polyelectrolyte P5) and a preparation method thereof. The structural formula of polyelectrolyte P5 is as follows:
[0114]
[0115] The synthetic route of polyelectrolyte P5 is as follows:
[0116]
[0117] The preparation method of polyelectrolyte P5 comprises the following steps:
[0118] Under the protection of inert gas, 53.2 mg of 1,1'-[1,2-bis[4-(2-phenylethynyl)phenyl]-1,2-vinyl]bisbenzene, 28.22 mg of 1,5-di(2-pyridyl)naphthalene, 18.5 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer and 203.21 mg of silver trifluoroacetate were added to 1 mL of dry acetonitrile solution for dissolution, and stirred for reaction at 120°C for 12 h. After the reaction was complete, the reaction mother liquor was diluted with 4 mL of dichloromethane and 1 mL of methanol, filtered through a 4 cm high neutral alumina column (200 mesh), and then directly precipitated in 100 mL of ether solution. The precipitate was collected and dried in vacuum at 65°C to constant weight to obtain polyelectrolyte P5 with a yield of 84.8%.
[0119] The H NMR spectrum of the polyelectrolyte P5 prepared in Example 5 in deuterated dimethyl sulfoxide is shown in Figure 8 As shown. Figure 8 It can be seen that the solvent peak and water peak of deuterated dimethyl sulfoxide are located at 2.50ppm and 3.30ppm respectively, and the solvent peak of residual dichloromethane is at 5.76ppm. In addition, all other signals are hydrogen atom signals of polyelectrolyte P5, and several characteristic hydrogen atom signals can also be assigned accordingly.
[0120] The photoluminescence curves of the polyelectrolyte P5 prepared in this example in dimethyl sulfoxide solutions with different water contents are shown in FIG. Fig. 9 As shown in (A), the fluorescence emission intensity variation trend of polyelectrolyte P5 in dimethyl sulfoxide solutions with different water contents is shown in Fig. 9 As shown in (B), I represents the photoluminescence intensity of polyelectrolyte P5 in dimethyl sulfoxide solutions with different water contents, I 0 represents the photoluminescence intensity of polyelectrolyte P5 in pure dimethyl sulfoxide. Fig. 9 As can be seen in (B), with the increase of water content, the fluorescence of polyelectrolyte P5 gradually increases and reaches a maximum at 90% water content, proving that the polyelectrolyte P5 exhibits obvious aggregation-induced emission phenomenon.
[0121] In summary, the present invention provides a main chain charged fused heterocyclic polyelectrolyte and its preparation method and application. The polyelectrolyte provided by the present invention is a polycyclic fused main chain charged fused heterocyclic polyelectrolyte, which has special aggregated luminescence performance, good solubility (such as being soluble in dichloromethane, methanol, acetonitrile, N,N-dimethylformamide, and dimethyl sulfoxide), film-forming property, excellent thermal stability and morphological stability, and has unique potential application value in the fields of optical devices and protein detection. In addition, the preparation method provided by the present invention is simple and efficient, and only one-step reaction, i.e., rhodium-catalyzed CH activation cyclization reaction, is required to obtain the target product. The raw materials used are cheap and easy to obtain, the yield is high (the yield is as high as 98.0%), the product is easy to separate, and it has high atom economy. The present invention effectively solves the problem that the charges of existing polyelectrolytes are mostly combined on the side chains of conjugated polymers, which is difficult to directly affect the electronic properties of the conjugated main chain, and has certain limitations in the regulation of photophysical properties.
[0122] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A main chain charged fused heterocyclic polyelectrolyte, characterized in that: The structural formula of the main chain charged fused heterocyclic polyelectrolyte is: Wherein, x, y, z, and w are each independently an integer between 1 and 200; R1 is aryl, aryl derivative, unsubstituted alkyl or substituted alkyl; R2 is an aryl group, an aryl derivative, a nitro group, a cyano group, an unsubstituted alkyl group, a substituted alkyl group, a sulfur atom, a selenium atom, a hydrogen atom, a halogen atom or a biologically active fragment, wherein the biologically active fragment comprises one of a terpenoid, a steroid, a fatty alcohol and a vitamin; is an aryl group or an aryl derivative; Selected from One of them.
2. The main chain charged fused heterocyclic polyelectrolyte according to claim 1, characterized in that: R1 is selected from one of the following structural formulas 1 to 25: Wherein, -* represents a connection; m, p, q, r are each independently an integer between 1 and 20; R and R' are each independently a hydrogen atom, a halogen atom, a sulfur atom, a selenium atom, a nitro group, a cyano group, an unsubstituted alkyl group, a substituted alkyl group, an aryl group, an aryl derivative or a biologically active fragment, wherein the biologically active fragment includes one of terpenes, steroids, fatty alcohols and vitamins; X is one of an oxygen atom, a sulfur atom and a selenium atom.
3. The main chain charged fused heterocyclic polyelectrolyte according to claim 1, characterized in that: R2 is selected from one of the following structural formulas 26 to 35: Among them, -* indicates a connection; s, t are each independently an integer between 0 and 20; R and R' are each independently a hydrogen atom, a halogen atom, a sulfur atom, a selenium atom, a nitro group, a cyano group, an unsubstituted alkyl group, a substituted alkyl group, an aryl group, an aryl derivative or a biologically active fragment, wherein the biologically active fragment includes one of terpenes, steroids, fatty alcohols and vitamins.
4. The main chain charged fused heterocyclic polyelectrolyte according to claim 1, characterized in that: Select one of the following structural formulas: -* indicates a connection.
5. A method for preparing the main chain charged fused heterocyclic polyelectrolyte according to claim 1, characterized in that: The steps include: Adding a bipyridine-substituted aromatic compound, an internal alkyne monomer, a rhodium catalyst and an additive into a solvent, and reacting to obtain the main chain charged fused heterocyclic polyelectrolyte; The structural formula of the bipyridine substituted aromatic compound is: The structural formula of the internal alkyne monomer is: R1 is aryl, aryl derivative, unsubstituted alkyl or substituted alkyl; R2 is an aryl group, an aryl derivative, a nitro group, a cyano group, an unsubstituted alkyl group, a substituted alkyl group, a sulfur atom, a selenium atom, a hydrogen atom, a halogen atom or a biologically active fragment, wherein the biologically active fragment comprises one of a terpenoid, a steroid, a fatty alcohol and a vitamin; is an aryl group or an aryl derivative; The additive includes one of silver trifluoroacetate, silver trifluoromethanesulfonate, silver p-toluenesulfonate and anhydrous copper acetate.
6. The preparation method according to claim 5, characterized in that: The rhodium catalyst includes dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer; and the solvent includes at least one of acetonitrile, methanol, 1,2-dichloroethane, N,N-dimethylformamide and dimethyl sulfoxide.
7. The preparation method according to claim 5, characterized in that: The molar ratio of the internal acetylene monomer, the bipyridine substituted aromatic compound, the rhodium catalyst and the additive is 1:(0.5-1.25):(0.1-0.5):(2.3-9.5); the reaction concentration of the internal acetylene monomer is 0.05-2 mol / L; The reaction conditions are: Inert gas atmosphere, reaction temperature is 100-140°C, and reaction time is 12-24h.
8. The preparation method according to claim 5, characterized in that: After the reaction, the following steps are further included before obtaining the main chain charged fused heterocyclic polyelectrolyte: The reaction solution obtained after the reaction is cooled to room temperature, and filtered to obtain a filtrate; The filtrate is added to a precipitant for precipitation, and then filtered and dried.
9. The preparation method according to claim 8, characterized in that: The precipitant comprises at least one of methanol, ether, acetone and n-hexane; R1 is selected from one of the following structural formulas 1 to 25, and R2 is selected from one of the following structural formulas 26 to 35, Selected from one of the following structural formulas 36 to 46: Wherein, -* represents a connection point; m, p, q, r are each independently an integer between 1 and 20; s and t are each independently an integer between 0 and 20; R and R' are each independently a hydrogen atom, a halogen atom, a sulfur atom, a selenium atom, a nitro group, a cyano group, an unsubstituted alkyl group, a substituted alkyl group, an aryl group, an aryl derivative or a biologically active fragment, wherein the biologically active fragment includes one of terpenes, steroids, fatty alcohols and vitamins.
10. Use of the main chain charged fused heterocyclic polyelectrolyte according to any one of claims 1 to 4 and / or the main chain charged fused heterocyclic polyelectrolyte prepared by the preparation method according to any one of claims 5 to 9 in the field of optical devices or protein detection.
Citation Information
Patent Citations
Selenium / tellurium-containing heterocyclic polymer as well as preparation method and conversion method thereof
CN113429575A
Preparation method and application of imidazole-containing fused heterocycle polymer and polyelectrolyte
CN114163634A
Polysubstituted nitrogen and sulfur-containing fused heterocycle polymer as well as preparation method and application thereof
CN116462843A
Fused heterocyclic ring polyelectrolyte containing nitrogen heterocyclic ring onium salt structure as well as preparation method and application of fused heterocyclic ring polyelectrolyte
CN117924697A
Cited By
Fused heterocyclic polymer, and preparation method therefor and use thereof
WO2026156950A1