Biodegradable copolyester PBCAT as well as preparation method and application thereof

By preparing biodegradable copolyester PBCAT, the problems of insufficient mechanical strength and degradation rate of traditional PBAT are solved, and it can be used in application scenarios with low hardness and long service life. It is suitable for soft products such as sealing strips and has excellent Flexibility and degradation properties.

CN118725271APending Publication Date: 2024-10-01SICHUAN UNIV +1

Patent Information

Application Number
CN202410937583.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional plastics are difficult to degrade naturally, resulting in a serious problem of "white pollution". The existing biodegradable material PBAT has deficiencies in mechanical strength and degradation rate, which limits its application scope.

Method used

A preparation method of biodegradable copolyester PBCAT is adopted, and 1,4-cyclohexanedimethanol, 1,4-butanediol, terephthalic acid, adipic acid and catalyst are mixed in the polyester through esterification reaction. The esterification reaction is carried out in the synthesis device, combined with the precondensation and polycondensation procedures, to prepare PBCAT with excellent flexibility and reduced hardness, which is suitable for application scenarios with low hardness and long service life.

Benefits of technology

It improves the mechanical strength and degradation rate of PBCAT and reduces the hardness, making it suitable for soft products such as sealing strips without sacrificing flexibility. It has lower hardness and good biodegradability and is suitable for large-scale promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725271A_ABST
    Figure CN118725271A_ABST
Patent Text Reader

Abstract

The invention discloses a biodegradable copolyester PBCAT and a preparation method and application thereof, and the biodegradable copolyester PBCAT is prepared by mixing three monomers of 1, 4-cyclohexanedimethanol, 1, 4-butanediol, terephthalic acid and adipic acid, then adding a catalyst and an antioxidant, and carrying out one-step melt polycondensation on all the mixtures. The copolyester PBCAT prepared by the preparation method provided by the invention not only has excellent mechanical properties, but also has excellent thermal stability, and the copolyester PBCAT prepared by the preparation method provided by the invention effectively solves the problem of narrow application field caused by high hardness and poor mechanical properties of traditional PBAT on the premise of keeping biodegradability, so that the copolyester PBCAT has wide application prospects. Meanwhile, the contradiction between the degradability and the good use performance of PBAT is balanced, the problem that use is affected due to the fact that the mechanical performance is obviously reduced due to the fact that degradation is fast in the use process of PBAT is solved, and the application value in the fields of elastomers, sealing materials and the like is remarkable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a biodegradable copolyester PBCAT and a preparation method and application thereof. Background Art

[0002] At present, global plastic consumption is growing at an annual rate of 8%, and the annual consumption of plastic will reach more than 700 million tons in 2030. However, traditional plastics have high chemical stability and are difficult to degrade naturally, resulting in an increasingly serious "white pollution" problem. According to the data listed at the 2018 International Biopolyester Conference, only 10% of traditional plastics are recycled, 12% are incinerated, and more than 70% of waste plastics are directly discarded in the natural environment, polluting the air, soil, oceans and water bodies, and even threatening human health. Therefore, in order to solve the problems of visual pollution, soil pollution, air pollution, marine pollution and microplastic pollution caused by waste plastics, the development of biodegradable plastics to replace traditional plastics has become a current research hotspot under the promotion of relevant policies issued by countries around the world.

[0003] Biodegradable materials generally refer to polymer materials that can be completely degraded into small molecules or water and carbon dioxide under natural conditions or other specific treatment conditions. Polybutylene terephthalate adipate (PBAT) is a biodegradable material that can be 100% degraded into small molecules such as water and carbon dioxide under certain conditions. At the same time, because PBAT is composed of butylene terephthalate structural units (BT) and butylene adipate structural units (BA), it has both excellent flexibility and good impact resistance. It is currently one of the most popular petroleum-based biodegradable materials with the best market application. Compared with biodegradable polyesters such as polylactic acid (PLLA) and polybutylene succinate (PBS), the mechanical properties of PBAT show stronger flexibility, and its elongation at break is above 700%. It also has excellent film-forming properties and easy blowing properties. However, compared with traditional plastics, PBAT has poor mechanical strength and high cost. At the same time, PBAT is a hard plastic with a Shore A hardness of 85 to 105, which cannot be used in the field of soft products. In addition, PBAT also has the problem that its mechanical properties will decrease due to degradation. Therefore, the application of PBAT is limited to disposable film products such as packaging materials (garbage bags and film packaging, etc.), medical products and agricultural mulch films. Summary of the invention

[0004] The purpose of the present invention is to provide a biodegradable copolyester PBCAT, which, compared with the existing PBAT, has improved mechanical strength, reduced hardness, and reduced degradation rate without sacrificing flexibility. It can be used in application scenarios with low hardness and long service life, and has potential application value in the field of soft products such as sealing strips.

[0005] In order to achieve the above object, the present invention provides a method for preparing a biodegradable copolyester PBCAT, comprising the following steps:

[0006] S1: placing 1,4-cyclohexanedimethanol, 1,4-butanediol, terephthalic acid, adipic acid, a catalyst and an antioxidant into a polyester synthesis device for esterification reaction;

[0007] S2: Perform pre-condensation until the water produced by the reaction is close to the theoretical value, and set the pre-condensation parameters and program to perform the pre-condensation reaction;

[0008] S3: After the pre-polycondensation is completed, a polycondensation program is set to carry out the polycondensation reaction, and after the completion, the product is discharged under the protection of an inert atmosphere;

[0009] The above theoretical values ​​are calculated based on the molar number of each component added in S1.

[0010] Preferably, the proportions of the components in the above S1 are: 5-65 parts of 1,4-cyclohexanedimethanol, 40-100 parts of 1,4-butanediol, 5-85 parts of terephthalic acid, 5-75 parts of adipic acid, 0.30-0.50 parts of catalyst, and 0.15-0.20 parts of antioxidant.

[0011] The present invention also provides an optimal ratio, which is specifically: 20.19 parts of 1,4-cyclohexanedimethanol monomer, 100.93 parts of 1,4-butanediol monomer, 52.33 parts of terephthalic acid monomer, 56.26 parts of adipic acid monomer, 0.26 parts of catalyst and 0.23 parts of antioxidant.

[0012] Preferably, the catalyst is selected from one or more of a titanium-based catalyst, a tin-based catalyst, and a zinc-based catalyst, preferably tetrabutyl titanate; the antioxidants are antioxidant 1010 and antioxidant 608, and the ratio thereof is preferably 1:1.

[0013] Preferably, the above esterification reaction is as follows: firstly, the air in the device is replaced with nitrogen three times, the reactants are heated to 80°C and maintained at this temperature for 0.5h to be fully mixed, and then the temperature is raised to 210°C for esterification reaction.

[0014] Preferably, the parameters and procedures of the above pre-condensation are: the temperature is set to rise to 230° C., at which time the pressure reaches 0.2 MPa, the vacuum pump is turned on to evacuate, and after 5 minutes, the pressure gradually drops to 2 kPa and is maintained for 40 minutes.

[0015] Preferably, the polycondensation procedure is as follows: heating the mixture to 265° C. and maintaining the system vacuum at 50 Pa for 4 hours.

[0016] The present invention also provides a biodegradable copolyester PBCAT prepared by the above preparation method.

[0017] The biodegradable copolyester PBCAT provided by the present invention can be used in the field of soft products, including the preparation of elastic sealing materials, etc.

[0018] The biodegradable copolyester PBCAT of the present invention has the following advantages:

[0019] 1) The copolyester PBCAT prepared by the present invention has good biodegradability and excellent flexibility, and at the same time, the non-planar rigid aliphatic ring structure of CHDM is used to solve the shortcomings of low strength, fast degradation rate and limited application of traditional PBAT.

[0020] 2) The method used in the present invention for preparing the copolyester PBCAT is a one-step direct esterification method, which is a typical representative technology for Chinese manufacturers to produce traditional PBAT. In industrial production, no special equipment and process flow are required, and it has great advantages in continuous production and controlling production costs.

[0021] 3) The copolyester PBCAT prepared by the present invention has a relatively low hardness (<85), meets the performance requirements of sealing strips of refrigerators, etc., can be applied to the field of soft products such as sealing strips, and has the prospect of large-scale promotion.

[0022] 4) The present invention provides an optimal ratio, that is, when the mass percentage of 1,4-cyclohexanedimethanol is about 8%, the mechanical properties of the copolyester PBCAT are suitable and the cost performance is the highest. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The copolyester PBCAT of Example 1 of the present invention 1 H-NMR analysis results.

[0024] Figure 2 This is the XRD analysis result of the copolyester PBCAT in Example 1 of the present invention.

[0025] Figure 3 This is the DSC analysis result of the copolyester PBCAT in Example 1 of the present invention.

[0026] Figure 4 The molecular structure formula of the copolyester PBCAT provided by the present invention is shown in FIG.

[0027] Figure 5 The mechanical properties analysis results of the copolyester PBCAT in Examples 1-6 of the present invention and the materials obtained in Comparative Examples 1-2 are shown.

[0028] Figure 6It is a thermal gravimetric loss (TGA) curve of the copolyester PBCAT in Examples 1-6 of the present invention and the PBAT in Comparative Example 1.

[0029] Figure 7 The scanning electron microscope images of the copolyester PBCAT in Examples 1-6 of the present invention and the PBAT in Comparative Example 1 after enzymatic degradation. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Note: The experimental methods in the following examples are conventional methods unless otherwise specified, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples are all commercially available unless otherwise specified.

[0032] Example 1

[0033] A one-step method for preparing biodegradable copolyester PBCAT is as follows:

[0034] Based on the mass parts calculated according to the set molar number (the same below), 20.19 parts of 1,4-cyclohexanedimethanol monomer, 100.93 parts of 1,4-butanediol monomer, 52.33 parts of terephthalic acid monomer, 56.26 parts of adipic acid monomer, 0.26 parts of catalyst and 0.23 parts of antioxidant were put into a 500mL polyester synthesis experimental device, wherein the catalyst was tetrabutyl titanate, and the antioxidant was 1:1 antioxidant 1010 and antioxidant 608.

[0035] After the reactor of the device was replaced with nitrogen for three times, the reactants were heated to 80°C and maintained at this temperature for 0.5h to fully mix, and then heated to 210°C for esterification reaction. When the water produced by the reaction was close to the theoretical value (calculated by the molar number of the feed), the pre-condensation process was carried out. The pre-condensation parameters and procedures were set, and the temperature was raised to 230°C. At this time, the pressure reached 0.2MPa, and the vacuum pump was turned on to evacuate. After 5min, the pressure gradually dropped to 2kPa and maintained for 40min. After the pre-condensation process, the mixture was heated to 265°C, and the system vacuum was maintained at 50Pa for 4h. Finally, the molten product sample was discharged under the protection of nitrogen to obtain the biodegradable copolyester PBCAT.

[0036] The obtained product was measured and its 1The results of H-NMR analysis are as follows Figure 1 As shown in A, the XRD analysis results are as follows Figure 2 The DSC curves of cooling (a) and reheating (b) after eliminating the thermal history are shown in Figure 3 shown.

[0037] Example 2

[0038] This embodiment provides another component ratio, and prepares the biodegradable copolyester PBCAT by a one-step method, which is as follows:

[0039] In terms of mass fractions, 5.05 parts of 1,4-cyclohexanedimethanol monomer, 110.40 parts of 1,4-butanediol monomer, 52.33 parts of terephthalic acid monomer, 56.26 parts of adipic acid monomer, 0.26 parts of catalyst and 0.23 parts of antioxidant were put into a 500mL polyester synthesis experimental device, wherein the components of the catalyst and antioxidant were the same as those in Example 1. The preparation process was the same as that in Example 1, and finally, the melted product sample was discharged under the protection of nitrogen.

[0040] The obtained product was measured and its 1 The results of H-NMR analysis are as follows Figure 1 As shown in B.

[0041] Example 3

[0042] This embodiment provides another component ratio, and prepares the biodegradable copolyester PBCAT by a one-step method, which is as follows:

[0043] In terms of mass fractions, 10.09 parts of 1,4-cyclohexanedimethanol monomer, 107.24 parts of 1,4-butanediol monomer, 52.33 parts of terephthalic acid monomer, 56.26 parts of adipic acid monomer, 0.26 parts of catalyst and 0.23 parts of antioxidant were put into a 500mL polyester synthesis experimental device, wherein the components of the catalyst and antioxidant were the same as those in Example 1. The preparation process was the same as that in Example 1, and finally, the melted product sample was discharged under the protection of nitrogen.

[0044] The obtained product was measured and its 1 The results of H-NMR analysis are as follows Figure 1 As shown in B.

[0045] Example 4

[0046] This embodiment provides another component ratio, and prepares the biodegradable copolyester PBCAT by a one-step method, which is as follows:

[0047] In terms of mass fractions, 15.14 parts of 1,4-cyclohexanedimethanol monomer, 104.09 parts of 1,4-butanediol monomer, 52.33 parts of terephthalic acid monomer, 56.26 parts of adipic acid monomer, 0.26 parts of catalyst and 0.23 parts of antioxidant were put into a 500mL polyester synthesis experimental device, wherein the components of the catalyst and antioxidant were the same as those in Example 1. The preparation process was the same as that in Example 1, and finally, the melted product sample was discharged under the protection of nitrogen.

[0048] The obtained product was measured and its 1 The results of H-NMR analysis are as follows Figure 1 As shown in B.

[0049] Example 5

[0050] This embodiment provides another component ratio, and prepares the biodegradable copolyester PBCAT by a one-step method, which is as follows:

[0051] In terms of mass fractions, 25.24 parts of 1,4-cyclohexanedimethanol monomer, 97.78 parts of 1,4-butanediol monomer, 52.33 parts of terephthalic acid monomer, 56.26 parts of adipic acid monomer, 0.26 parts of catalyst and 0.23 parts of antioxidant were put into a 500mL polyester synthesis experimental device, wherein the components of the catalyst and antioxidant were the same as those in Example 1. The preparation process was the same as that in Example 1, and finally, the melted product sample was discharged under the protection of nitrogen.

[0052] The obtained product was measured and its 1 The results of H-NMR analysis are as follows Figure 1 As shown in B.

[0053] Example 6

[0054] This embodiment provides another component ratio, and prepares the biodegradable copolyester PBCAT by a one-step method, which is as follows:

[0055] In terms of mass fractions, 30.28 parts of 1,4-cyclohexanedimethanol monomer, 94.63 parts of 1,4-butanediol monomer, 52.33 parts of terephthalic acid monomer, 56.26 parts of adipic acid monomer, 0.26 parts of catalyst and 0.23 parts of antioxidant were put into a 500mL polyester synthesis experimental device, wherein the components of the catalyst and antioxidant were the same as those in Example 1. The preparation process was the same as that in Example 1, and finally, the melted product sample was discharged under the protection of nitrogen.

[0056] The obtained product was measured and its 1 The results of H-NMR analysis are as follows Figure 1 As shown in B.

[0057] Comparative Example 1

[0058] This comparative example provides a method for preparing PBAT by a one-step process, which is as follows:

[0059] In terms of mass fractions, 113.55 parts of 1,4-butanediol monomer, 52.33 parts of terephthalic acid monomer, 56.26 parts of adipic acid monomer, 0.26 parts of catalyst and 0.23 parts of antioxidant were put into a 500mL polyester synthesis experimental device, wherein the components of the catalyst and antioxidant were the same as those in Example 1. The preparation process was the same as that in Example 1, and finally, the melted product sample was discharged under the protection of nitrogen.

[0060] The obtained product was measured and its 1 The results of H-NMR analysis are as follows Figure 1 As shown in B.

[0061] Comparative Example 2

[0062] This comparative example provides a method for preparing PBCAT by a two-step transesterification method, which is as follows:

[0063] In parts by mass, 52.33 parts of terephthalic acid monomer, 10.08 parts of 1,4-cyclohexanedimethanol monomer, 50.47 parts of 1,4-butanediol monomer, 0.10 parts of catalyst and 0.10 parts of antioxidant were put into a 500mL polyester synthesis experimental device, the reaction temperature was 210°C, and the reaction was carried out under the protection of a nitrogen atmosphere for 4 hours; then 56.26 parts of adipic acid monomer, 10.08 parts of 1,4-cyclohexanedimethanol monomer, 50.47 parts of 1,4-butanediol monomer, 0.10 parts of catalyst and 0.10 parts of antioxidant were respectively put into a 500mL polyester synthesis experimental device, the reaction temperature was 190°C, and the reaction was carried out under the protection of a nitrogen atmosphere for 4 hours, and the components of the catalyst and antioxidant were the same as those in Example 1.

[0064] After the two esterification reactions were completed, the two esterification products were mixed evenly, and 0.20 parts of stannous octoate [Sn(Oct)2] was used as a polycondensation catalyst. The temperature was maintained at 230°C for 40 minutes, and the pressure gradually dropped to 2 kPa. After the pre-polycondensation process was completed, the mixture was heated to 265°C, and the system vacuum was maintained at 50 Pa for 4 hours. Finally, the molten sample was discharged under the protection of nitrogen.

[0065] right Figure 1 of 1H-NMR test results are analyzed. In the process of melt polycondensation, a large number of ester bonds are formed between diols and dibasic acids in PBACT copolyester. The hydrogen protons on the methylene groups directly connected to the ester bonds will form split peaks with different chemical shifts due to the different polarities of the adjacent diacids and diols. The peak range of these split peaks is between 3.80ppm and 4.55ppm. The chemical structure of PBCAT copolyester can be inferred by analyzing them. 1 H-NMR Figure 1 A in the synthesis of PBCAT copolyester, the amount of 1,4-BDO used is greater than that of CHDM, see Figure 1 As shown in A in the figure, the four broad and strong peaks a (4.44ppm), b (4.38ppm), c (4.15ppm) and d (4.09ppm) correspond to the four structural units TBT, TBA, ABT and ABA respectively; 4.19ppm is the f-number methylene hydrogen proton peak on the TCT structural unit formed by CHDM and PTA; 4.25-4.32ppm is the e-number methylene hydrogen proton peak on the TCA and ACT structural units formed by CHDM on one side and PTA; 3.96-4.05ppm is the g-number methylene hydrogen proton peak on the ACT and TCA structural units formed by CHDM on one side and AA; 3.90ppm is the h-number methylene hydrogen proton peak on the ACA structural unit formed by CHDM and AA, so the structural formula of PBCAT copolyester can be obtained as follows: Figure 4 shown.

[0066] By integrating the peaks of 'a~h' in PBCAT copolyester, the actual proportions of PTA and AA, BDO and CHDM can be obtained, as shown in Table 1 below. The actual proportions are basically consistent with the feed ratio; with the increase of the amount of CHDM introduced, the average sequence length of the aromatic structural unit (L T ), the average sequence length of aliphatic structural units (L A ) all increase to varying degrees, which will affect the thermal stability of the copolyester. With the increase of CHDM content, the R value of the copolyester decreases accordingly (<1), which shows that the molecular chain conformation of the copolyester is relatively tight and orderly, which may affect certain properties of the copolyester, such as increased mechanical strength.

[0067] Table 1 Proportion of each structural unit of PBCAT copolyester

[0068]

[0069]

[0070] Experimental Example 1

[0071] This test example measures the properties of the products obtained in the above examples and comparative examples, as follows:

[0072] 1. Determination of mechanical properties

[0073] (1) Hardness test: The samples of Examples 1-6 and Comparative Examples 1-2 were prepared into 3 cm × 4 cm × 6 mm specimens by compression molding. According to GB / T 531.1-2008 "Test method for indentation hardness of vulcanized rubber or thermoplastic rubber Part 1: Shore hardness", the Shore hardness tester A was used for measurement. Each group of specimens was measured 5 times and the average value was taken. The hardness test results of all product materials were obtained as follows: Figure 5 As shown in a in .

[0074] (2) Tensile property test: According to the test standard GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets", the samples of Examples 1-6 and Comparative Examples 1-2 were prepared into 5cm×4cm×1mm dumbbell-shaped standard tensile specimens by compression molding, and tested at room temperature using an Instron 5567 universal material testing machine. The tensile rate was set to 50mm / min and the original gauge length was 25mm. The tensile strength and elongation at break of all product samples were measured, and the average of the test results of 5 specimens was finally taken. The tensile property test results of all product materials are obtained as follows: Figure 5 As shown in b.

[0075] The three mechanical properties of all product samples were measured and statistically analyzed, and the results are shown in Table 2.

[0076] Table 2 Test results of tensile strength, elongation at break and hardness of samples

[0077]

[0078] It can be seen from the results in Table 2 that the mechanical properties of the material can be improved by introducing CHDM with a rigid structure. In Example 1, the amount of CHDM added is 20.19 parts, and the copolyester has the best mechanical properties, the hardness is reduced to 80 Shore A, the tensile strength gradually increases from 7.20 MPa to 11.41 MPa, and the elongation at break increases from 274% to 957%. Therefore, the PBCAT copolyester obtained in this patent realizes the application of biodegradable materials to soft products such as sealing materials for the first time, such as the preparation of sealing materials and elastomeric materials.

[0079] 2. Thermal stability performance determination

[0080] The test was conducted using a TG209F1 from NETZSCH, Germany, under nitrogen atmosphere, a heating rate of 10°C / min, and a temperature range of 0 to 800°C.

[0081] After measurement, the thermal gravimetric temperature (TGA) curves of the products obtained in Examples 1-6 and Comparative Example 1 are as follows: Figure 6 As shown, the 5% thermal weight loss temperature (T -5% )、10% thermal weight loss temperature (T -10% ) and the maximum thermal weight loss temperature (T max The thermogravimetric analysis test results of ) are shown in Table 3.

[0082] Table 3 Thermogravimetric analysis results of samples

[0083]

[0084] From the results in Table 3, we can see that T -5% 、T -10% and T max The value shows a slightly increasing trend with the increase of CHDM content. Therefore, the introduction of CHDM improves the rigidity of the PBCAT copolyester molecular chain, which is beneficial to improving the thermal stability of the modified copolyester.

[0085] 3. Degradation performance determination

[0086] The samples of Examples 1-6 and Comparative Example 1 were prepared into thin sheets of certain specifications (thickness 1 mm, size 10 mm×10 mm) by compression molding. The sample sheets and 5 mL of 0.1 M phosphate buffer solution (pH=7.2) containing lipase (0.025 mg / mL) were placed in a tube. The samples were then placed in a 30°C constant temperature shaker for 84 days. The degradation solution was replaced every 7 days and each sample was taken out. The samples were washed with deionized water and dried in a vacuum oven to constant weight. The remaining mass of the samples was weighed and recorded, and the degradation rate was calculated after 140 days of degradation. Scanning electron microscope images of each product after enzyme degradation are shown in Figure 2. Figure 7 ,in Figure 7 ag in the figure are respectively the electron microscope scanning conditions of Examples 1, 2 to 6 and Comparative Example 1, and a-1 to g-1 in the figure are respectively the magnified images of the marked positions. The degradation rates of the above samples after enzymatic hydrolysis are measured and shown in Table 4.

[0087] Table 4 Degradation rate test results of samples

[0088]

[0089] From the results in Table 4, it can be seen that when the degradation time reaches 140 days, the mass loss of PBCAT-0 and PBCAT-0.05 is close to 12%, while the mass loss of PBCAT-0.20, PBCAT-0.25 and PBCAT-0.30 samples is about 4%. The introduction of CHDM can significantly reduce the degradation rate of PBCAT copolyester. This patent studies the degradation behavior of PBCAT copolyester for the first time and finds that the development of PBCAT can effectively solve the inherent contradiction between the degradability and good performance of traditional PBAT.

[0090] By comparing the above results, wherein, compared with Comparative Example 2, in process flow, the two-step process flow of Comparative Example 2 is complicated, and it is necessary to increase additional process equipment and it is impossible to achieve continuous production, so in industrial production, Example 1 has more advantages; in material performance, the tensile strength of the two is not much different, but the elongation at break of Example 1 is significantly better than Comparative Example 2, and the lower hardness of Example 1 can meet more application scene requirements; in catalyst, Example 2 uses a tin catalyst in the polycondensation stage, and the catalyst is easy to lose activity under the conditions of water and oxygen, so it is more demanding to the reaction conditions, because the tin catalyst has certain toxicity and danger, it is necessary to post-process it, otherwise it will cause environmental pollution, therefore using one-step synthesis PBCAT has obvious advantages. Compared with Comparative Example 1, the tensile strength of Example 1 is significantly improved, and the elongation at break is significantly increased, and the Shore A hardness is significantly reduced, and the degradation rate is moderate (having both degradation performance and good use performance), and it can be seen that the performance of the product in Example 1 is the best.

[0091] In summary, the present invention provides a method for preparing a biodegradable copolyester PBCAT. Compared with the existing PBAT, the biodegradable copolyester PBCAT prepared by the method has improved mechanical strength, reduced hardness, and slowed degradation rate without sacrificing flexibility. It can be used in application scenarios with low hardness and long service life, and has obvious application prospects in the field of soft products such as sealing strips.

[0092] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A method for preparing a biodegradable copolyester PBCAT, characterized in that: The following steps are involved: S1: placing 1,4-cyclohexanedimethanol, 1,4-butanediol, terephthalic acid, adipic acid, a catalyst and an antioxidant into a polyester synthesis device for esterification reaction; S2: Perform pre-condensation until the water produced by the reaction is close to the theoretical value, and set the pre-condensation parameters and program to perform the pre-condensation reaction; S3: After the pre-polycondensation is completed, a polycondensation program is set to carry out the polycondensation reaction, and after the completion, the product is discharged under the protection of an inert atmosphere; The theoretical value is calculated by the molar number of each component added in S1.

2. The preparation method according to claim 1, characterized in that: The proportions of the components in S1 are: 5-65 parts of 1,4-cyclohexanedimethanol, 40-100 parts of 1,4-butanediol, 5-85 parts of terephthalic acid, 5-75 parts of adipic acid, 0.30-0.50 parts of catalyst, and 0.15-0.20 parts of antioxidant.

3. The preparation method according to claim 2, characterized in that: The ratio is: 20.19 parts of 1,4-cyclohexanedimethanol monomer, 100.93 parts of 1,4-butanediol monomer, 52.33 parts of terephthalic acid monomer, 56.26 parts of adipic acid monomer, 0.26 parts of catalyst and 0.23 parts of antioxidant.

4. The preparation method according to claim 1, characterized in that: The catalyst is selected from one or more of a titanium catalyst, a tin catalyst, and a zinc catalyst; the antioxidant is antioxidant 1010 and antioxidant 608.

5. The preparation method according to claim 4, characterized in that: The catalyst is selected from tetrabutyl titanate; the ratio of antioxidant 1010 to antioxidant 608 in the antioxidant is 1:

1.

6. The preparation method according to claim 1, characterized in that: The esterification reaction is as follows: firstly, the air in the device is replaced with nitrogen three times, the reactants are heated to 80°C and maintained at this temperature for 0.5h to be fully mixed, and then the temperature is raised to 210°C for esterification reaction.

7. The preparation method according to claim 1, characterized in that: The parameters and procedures of the pre-condensation are as follows: the temperature is set to rise to 230° C., at which time the pressure reaches 0.2 MPa, the vacuum pump is turned on to evacuate, and after 5 minutes, the pressure gradually drops to 2 kPa and is maintained for 40 minutes.

8. The preparation method according to claim 1, characterized in that: The polycondensation procedure is as follows: the mixture is heated to 265° C. and the system vacuum is maintained at 50 Pa for 4 hours.

9. A biodegradable copolyester PBCAT prepared by the preparation method according to any one of claims 1 to 8.

10. The use of the biodegradable copolyester PBCAT as claimed in claim 9 in the field of soft products, characterized in that: The application includes the preparation of elastic sealing materials.

Citation Information

Patent Citations

  • Preparation method of copolyether ester

    CN101735436A

  • Thermoplastic block copolyether ester elastomer and preparation method thereof

    CN101747499A

  • Aliphatic / aromatic copolyester and preparation method thereof

    CN102485765A

  • Method for continuously preparing biodegradable plastic

    CN102558515A

  • High-transparency PBAT degradable copolyester and preparation method thereof

    CN115716909A

Cited By

  • PET modified atmosphere food packaging material and preparation method thereof