Copolyamide material as well as preparation method and application thereof
By introducing a long carbon chain structure and a specific proportion of long carbon chain amide salts into polyamide 66, the strength and toughness of polyamide 66 are improved, the problem of performance degradation in humid environments is solved, and dimensional stability and impact toughness are achieved. The improvement is suitable for a variety of application fields.
Patent Information
- Application Number
- CN202310338470.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-31
AI Technical Summary
The strength and toughness of existing polyamide 66 materials decrease in humid environments, and the dimensional stability is poor. Existing modification methods fail to fully improve its performance in humid environments.
By introducing a long carbon chain structure into polyamide 66, reducing the proportion of amide groups, introducing long methine chains that can be freely stretched and rotated, and using a specific proportion of polyamide 66 salts and long carbon chain amide salts for copolymerization, the material is improved. strength, toughness and dimensional stability.
It achieves high strength and toughness in humid environments, improves the dimensional stability and impact toughness of the material, and is suitable for electronic appliances, automobiles, home appliances and other fields.
Smart Images

Figure BDA0004157306970000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a copolyamide material and a preparation method and application thereof. Background Art
[0002] Polyamide 66 (PA66) is a thermoplastic resin with high mechanical strength, hardness and rigidity. It can be used as an engineering plastic and is widely used in mechanical accessories such as gears and lubricated bearings. In addition, polyamide 66 also has excellent hygroscopicity and can be used in humid environments. However, it is precisely because of its excellent hygroscopicity that when it is used in a humid environment, its strength and toughness decrease and its dimensional stability deteriorates due to the influence of moisture absorption. Therefore, how to improve the strength and toughness of polyamide 66 in a humid environment and maintain its dimensional stability is a problem that people are more concerned about.
[0003] In the prior art, polyamide 66 is often modified to reduce its water absorption rate and improve its strength and toughness. For example, CN102226036A discloses a calcium sulfate corn starch polyamide 66 composite material and its preparation process; the composite material is made of the following raw materials in weight percentage: calcium sulfate 15-50wt%, corn starch 10-40wt%, polyamide 66 20-60wt%, heat stabilizer T-68 1-10w%, antioxidant 10101-10wt% and stearic acid 1-20wt%. PA66 is modified by using corn starch and calcium sulfate to reduce its water absorption rate. However, the toughness of the composite material needs to be further improved.
[0004] For example, CN103044913A discloses an in-situ compatibilization preparation of super-tough polyamide 66 nanocomposite material and its preparation method; the polyamide 66 nanocomposite material comprises polyamide 66, EPDM rubber, initiator, maleic anhydride and organic montmorillonite. The super-tough polyamide 66 nanocomposite material has good low-temperature impact resistance and low water absorption; however, the strength needs to be further improved.
[0005] Therefore, it is a technical problem to be urgently solved in the art to provide a copolyamide material having excellent tensile strength, excellent bending strength, compressive strength, good toughness, and good dimensional stability, or having excellent impact toughness, good elongation at break, good dimensional stability, and no significant decrease in tensile strength. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention aims to provide a copolyamide material and a preparation method and application thereof. The copolyamide material uses polyamide 66 salt and long carbon chain amide salt as raw materials, introduces a long carbon chain structure into polyamide 66, so that the product has good strength and toughness and good dimensional stability.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a copolyamide material, wherein raw materials of the copolyamide material include polyamide 66 salt and long carbon chain amide salt.
[0009] In the present invention, specific raw materials are selected to introduce a long carbon chain structure into the molecular structure of polyamide 66, thereby reducing the proportion of amide groups in the copolymer, thereby weakening the hygroscopicity of polyamide 66 and improving its dimensional stability; at the same time, the introduction of the long carbon chain structure provides the copolymer with a long methyl chain that can stretch and rotate freely, thereby improving the toughness and softness of the product, so that the polyamide has higher impact toughness, softness and strength at a lower temperature, and good dimensional stability.
[0010] Preferably, the mass ratio of the polyamide 66 salt to the long carbon chain amide salt is (0.1-9):1, for example, 0.1:1, 0.15:1, 0.2:1, 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, 0.55:1, 0.6:1, 0.65:1, 0.7:1, 0.75:1, 0.8:1, 0.85:1, 0.9:1, 0.95:1, 1:1, 1.2:1, 1.4:1, 1.6:1, 1.8:1, 2:1, 2.2: 1, 2.4:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1, 4.2:1, 4.4:1, 4.6:1, 4.8:1, 5:1, 5.2:1, 5.4:1, 5.6:1, 5.8:1, 6:1, 6.2:1, 6.4:1, 6.6:1, 6.8:1, 7:1, 7.2:1, 7.4:1, 7.6:1, 7.8:1, 8:1, 8.2:1, 8.4:1, 8.6:1, 8.8:1, 9:1, etc.
[0011] In the present invention, the mass ratio of the polyamide 66 salt to the long carbon chain amide salt is in the range of greater than 1:1 and less than or equal to 9:1, preferably (2-8):1, so that the copolyamide material has excellent tensile strength, can have good strength and toughness, good dimensional stability, and can be used as a modified base material in the fields of electronic appliances, automobiles and home appliances; the mass ratio of the polyamide 66 salt to the long carbon chain amide salt is in the range of (0.1-1):1, preferably (0.2-0.8):1, so that the copolyamide material has excellent impact toughness (including simply supported beam impact strength) and dimensional stability, can have good elongation at break, and tensile strength is not significantly deteriorated, and can be used as a modified base material in the fields of precision machinery parts, powder coatings, transmission gears, and coatings of wires and cables.
[0012] Preferably, the raw materials of the polyamide 66 salt include adipic acid and hexamethylenediamine. In the present invention, the preparation method of the polyamide 66 salt is not limited, and it can be prepared by a conventional method. For example, hexamethylenediamine and adipic acid are dissolved in a solvent respectively, and then the two solutions are mixed, cooled, separated, washed, and dried to obtain the polyamide 66 salt;
[0013] Alternatively, hexamethylenediamine and adipic acid are directly mixed in water to prepare a saturated aqueous solution, and after adjusting the pH value of the solution, the solution is cooled, separated, and dried to obtain polyamide 66 salt;
[0014] Alternatively, adipic acid is heated to a temperature above the melting point of hexamethylenediamine and below the melting point of adipic acid, and diamine is heated to a temperature above the melting point, and liquid hexamethylenediamine is added to the adipic acid by spraying to directly obtain polyamide 66 salt.
[0015] Preferably, the raw materials of the long carbon chain amide salt include long carbon chain dibasic acid and diamine.
[0016] Preferably, the number of carbon atoms in the long carbon chain dibasic acid is ≥10, for example, it can be 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, etc.
[0017] Preferably, the long carbon chain polyacid comprises at least one of sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid or pentadecanedioic acid.
[0018] Preferably, the diamine includes C4-C14 alkyl diamine, for example, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14 alkyl diamine, etc., wherein the C4-C14 alkyl diamine does not include hexamethylenediamine.
[0019] Preferably, the diamine includes at least one of butanediamine, pentamethylenediamine, heptanediamine, octanediamine, decanediamine, undecanediamine, dodecanediamine, and tridecanediamine.
[0020] In the examples of the present invention, pentamethylenediamine is selected, and the obtained copolyamide material not only has good performance (including strength) but also has low cost.
[0021] In the present invention, the long carbon chain amide salt refers to a raw material selected from long carbon chain dibasic acids, that is, dibasic acids with 10 to 20 carbon atoms.
[0022] In the present invention, the preparation method of the long-chain amide salt is not limited and can be prepared by conventional methods. Exemplarily, the method comprises: sequentially adding water, diamine and long-chain dibasic acid into a salt-forming tank for salt-forming reaction to obtain the long-chain amide salt.
[0023] In a second aspect, the present invention provides a method for preparing the copolyamide material according to the first aspect, the preparation method comprising the following steps:
[0024] The polyamide 66 salt is reacted with the long carbon chain amide salt to obtain the copolyamide material.
[0025] Preferably, the polyamide 66 salt exists in the form of polyamide 66 salt solution.
[0026] Preferably, the pH value of the polyamide 66 salt solution is 7.10-7.70, for example, it can be 7.10, 7.20, 7.30, 7.40, 7.50, 7.60, 7.70, etc.; the concentration of the polyamide 66 salt solution is 50-65%, for example, it can be 52%, 54%, 56%, 58%, 60%, 62%, 64%, etc.
[0027] Preferably, the long-chain amide salt exists in the form of a long-chain amide salt liquid.
[0028] Preferably, the pH value of the long-chain amide salt solution is 8.00-8.80, for example, 8.10, 8.20, 8.30, 8.40, 8.50, 8.60, 8.70, 8.80, etc.; the concentration of the long-chain amide salt solution is 60-70%, for example, 60%, 62%, 64%, 66%, 68%, 70%, etc.
[0029] Preferably, the reaction comprises a pressure increasing stage, a pressure maintaining stage, a pressure reducing stage and a post-polymerization stage which are performed in sequence.
[0030] Preferably, the duration of the pressure boost stage is 20 to 40 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, etc.
[0031] Preferably, the pressure in the pressure holding stage is 1.4-1.8 MPa, for example, it can be 1.4 MPa, 1.45 MPa, 1.5 MPa, 1.55 MPa, 1.6 MPa, 1.65 MPa, 1.7 MPa, 1.75 MPa, 1.8 MPa, etc.
[0032] Preferably, the initial temperature of the pressure holding stage is 200-250°C, for example, it can be 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 245°C, 250°C, etc.; the time of the pressure holding stage is 1-3h, for example, it can be 1h, 1.5h, 2h, 2.5h, 3h, etc.
[0033] Preferably, the pressure reduction stage lasts for 40 to 80 min, for example, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, etc.; the pressure is reduced to -0.002 to -0.03 MPa, for example, -0.02 MPa, -0.01 MPa, -0.005 MPa, -0.002 MPa, etc.
[0034] Preferably, the pressure in the post-polymerization stage is -0.005 to -0.02 MPa, for example, -0.005 MPa, -0.01 MPa, -0.015 MPa, -0.02 MPa, etc.
[0035] Preferably, the temperature of the post-polymerization stage is 230-270°C, for example, 230°C, 235°C, 240°C, 245°C, 250°C, 255°C, 260°C, 265°C, 270°C, etc.
[0036] Preferably, the duration of the post-polymerization stage is 20 to 40 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, etc.
[0037] In the present invention, the reaction is carried out in the presence of a protective atmosphere, which includes but is not limited to nitrogen.
[0038] As a preferred technical solution of the present invention, the preparation method comprises:
[0039] The polyamide 66 salt solution and the long carbon chain amide salt solution are introduced into a closed reactor, and the pressure in the reactor is increased to 1.4-1.8MPa and the temperature is increased to 200-250°C within 20-40min, and the pressure is maintained for 1-3h, and then the pressure is reduced to -0.002-0.02MPa within 40-80min, and then the post-polymerization stage is entered, and the reaction is carried out at a pressure of -0.005-0.02MPa and a temperature of 230-270°C for 20-40min to obtain the copolyamide material.
[0040] In the present invention, the copolyamide resin raw materials are polyamide 66 salt solution and long carbon chain amide salt solution, which are salted in parallel and then introduced into a reactor for polymerization to obtain copolyamide. The parallel salting method is conducive to precise control of a variety of salt solution raw materials and is conducive to obtaining a copolymer product with small viscosity fluctuation.
[0041] In a third aspect, the present invention provides a modified base material, wherein the modified base material comprises the copolyamide material as described in the first aspect.
[0042] Preferably, the modified base material is used in the fields of electronic appliances, automobiles, and household appliances.
[0043] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] The copolyamide material provided by the present invention uses polyamide 66 salt and long carbon chain amide salt as raw materials, introduces a long carbon chain structure into polyamide 66, so that polyamide 66 still has good strength and toughness and good dimensional stability in a humid environment. DETAILED DESCRIPTION
[0046] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0047] Example 1
[0048] The present embodiment provides a copolyamide material, wherein the raw materials of the copolyamide material include polyamide 66 salt and long-chain amide salt; the mass ratio of the polyamide 66 salt (PA66 salt) to the long-chain amide salt (PA510 salt) is 7.5:2.5; the raw materials of the polyamide 66 salt include adipic acid and hexamethylenediamine; the raw materials of the long-chain amide salt solution include sebacic acid and pentamethylenediamine.
[0049] This embodiment provides a method for preparing a copolyamide material, the preparation method comprising the following steps:
[0050] Under nitrogen protection, hexamethylenediamine, adipic acid and water are prepared into a PA66 salt solution, and the pH value of the PA66 salt solution is 7.30 and the concentration is 60% by controlling the ratio of adipic acid to hexamethylenediamine; sebacic acid, pentamethylenediamine and water are prepared into a PA510 salt solution, and the pH value of the PA510 salt solution is 8.40 and the concentration is 65% by controlling the ratio of sebacic acid to pentamethylenediamine; the PA66 salt solution and the PA510 salt solution are mixed and introduced into a reactor, and the pressure in the reactor is increased to 1.65MPa within 30min, and the material temperature is increased to 210°C. After maintaining the pressure for 1.5h under this condition, the material temperature is increased to 240°C, and then the pressure reduction stage is entered, and the pressure in the reactor is reduced to -0.013MPa within 60min and the temperature reaches 255°C, and then the post-polymerization stage is entered to continue the reaction for 30min to obtain the copolyamide material.
[0051] Example 2
[0052] The present embodiment provides a copolyamide material, wherein the raw materials of the copolyamide material include polyamide 66 salt and long carbon chain amide salt; the mass ratio of the polyamide 66 salt to the long carbon chain amide salt (PA512 salt) is 8:2; the raw materials of the polyamide 66 salt include adipic acid and hexamethylenediamine; the raw materials of the long carbon chain amide salt include dodecanedioic acid and pentamethylenediamine.
[0053] This embodiment provides a method for preparing a copolyamide material, and the specific steps of the preparation method are the same as those of Embodiment 1.
[0054] Example 3
[0055] This embodiment provides a copolyamide material, the raw materials of the copolyamide material include polyamide 66 salt and long carbon chain amide salt; the mass ratio of the polyamide 66 salt and the long carbon chain amide salt (PA510 salt) is 8.65:1.35; the raw materials of the polyamide 66 salt include adipic acid and hexamethylenediamine; the raw materials of the long carbon chain amide salt solution include sebacic acid and pentamethylenediamine.
[0056] This embodiment provides a method for preparing a copolyamide material, and the specific steps of the preparation method are the same as those of Embodiment 1.
[0057] Example 4
[0058] This embodiment provides a copolyamide material, wherein the raw materials of the copolyamide material include polyamide 66 salt and long carbon chain amide salt; the mass ratio of the polyamide 66 salt and the long carbon chain amide salt is 9:1; the raw materials of the polyamide 66 salt include adipic acid and hexamethylenediamine; the raw materials of the long carbon chain amide salt include sebacic acid and pentamethylenediamine.
[0059] This embodiment provides a method for preparing a copolyamide material, the preparation method comprising the following steps:
[0060] Under nitrogen protection, hexamethylenediamine, adipic acid and water are prepared into PA66 salt solution, and the pH value of the PA66 salt solution is 7.20 and the concentration is 55% by controlling the ratio of adipic acid to hexamethylenediamine; sebacic acid, pentamethylenediamine and water are prepared into PA510 salt solution, and the pH value of the PA510 salt solution is 8.70 and the concentration is 70% by controlling the ratio of sebacic acid to pentamethylenediamine; the PA66 salt solution and the PA510 salt solution are mixed and introduced into a reactor, and the pressure in the reactor is increased to 1.75MPa within 25min, and the material temperature is increased to 215°C. After maintaining the pressure for 1h under this condition, the material temperature is increased to 250°C, and then the pressure reduction stage is entered, and the pressure in the reactor is reduced to -0.03MPa within 45min, and the temperature reaches 265°C, and the reaction is continued for 20min in the post-polymerization stage to obtain the copolyamide material.
[0061] Example 5
[0062] This embodiment provides a copolyamide material, wherein the raw materials of the copolyamide material include polyamide 66 salt and long-chain amide; the mass ratio of the polyamide 66 salt to the long-chain amide salt is 6:5; the raw materials of the polyamide 66 salt include adipic acid and hexamethylenediamine; the raw materials of the long-chain amide salt include sebacic acid and pentamethylenediamine.
[0063] This embodiment provides a method for preparing a copolyamide material, the preparation method comprising the following steps:
[0064] Under nitrogen protection, hexamethylenediamine, adipic acid and water are prepared into PA66 salt solution, and the pH value of the PA66 salt solution is 7.70 and the concentration is 65% by controlling the ratio of adipic acid to hexamethylenediamine; sebacic acid, pentamethylenediamine and water are prepared into PA510 salt solution, and the pH value of the PA510 salt solution is 8.10 and the concentration is 60% by controlling the ratio of sebacic acid to pentamethylenediamine; the PA66 salt solution and the PA510 salt solution are mixed and introduced into a reactor, the pressure in the reactor is increased to 1.55MPa within 35min, the material temperature is increased to 205℃, and after maintaining the pressure for 2h under this condition, the material temperature is increased to 230℃, and then the pressure reduction stage is entered, the pressure in the reactor is reduced to -0.005MPa within 75min, and the temperature reaches 245℃, and the reaction is continued for 40min in the post-polymerization stage to obtain the copolyamide material.
[0065] Example 6
[0066] This embodiment provides a copolyamide material, which is different from Embodiment 5 only in that the total amount of the PA66 salt and the PA510 salt remains unchanged, with a mass ratio of 5:5, and the types, amounts and preparation methods of other raw materials are the same as those in Embodiment 5.
[0067] Example 7
[0068] This embodiment provides a copolyamide material, which is different from Embodiment 1 only in that the total amount of the PA66 salt and the PA510 salt remains unchanged, with a mass ratio of 10:1, and other raw material types, amounts and preparation methods are the same as those in Embodiment 1.
[0069] Example 8
[0070] This embodiment provides a copolyamide material, which is different from Embodiment 1 only in that the total amount of the PA66 salt and the PA510 salt remains unchanged, with a mass ratio of 0.08:1, and other raw material types, amounts and preparation methods are the same as those in Embodiment 1.
[0071] Example 9
[0072] This embodiment provides a copolyamide material, which is different from Embodiment 1 only in that the total amount of the PA66 salt and the PA510 salt remains unchanged, with a mass ratio of 0.65:1, and other raw material types, amounts and preparation methods are the same as those in Embodiment 1.
[0073] Example 10
[0074] This embodiment provides a copolyamide material, which is different from Embodiment 1 only in that the total amount of the PA66 salt and the PA510 salt remains unchanged, with a mass ratio of 0.55:1, and other raw material types, amounts and preparation methods are the same as those in Embodiment 1.
[0075] Embodiment 11
[0076] This embodiment provides a copolyamide material, which is different from Embodiment 1 only in that the total amount of the PA66 salt and the PA510 salt remains unchanged, with a mass ratio of 0.4:1, and other raw material types, amounts and preparation methods are the same as those in Embodiment 1.
[0077] Example 12
[0078] This embodiment provides a copolyamide material, which is different from the first embodiment only in that the sebacic acid is replaced by an equimolar amount of suberic acid, and the other raw material types, amounts and preparation methods are the same as those in the first embodiment.
[0079] Embodiment 13
[0080] This embodiment provides a copolyamide material, which differs from Embodiment 1 only in that the sebacic acid is replaced by an equimolar amount of hexadecanedioic acid, and other raw material types, amounts and preparation methods are the same as those in Embodiment 1.
[0081] Embodiment 14
[0082] This embodiment provides a copolyamide material, which is different from the first embodiment only in that the pentamethylenediamine is replaced by an equimolar amount of hexamethylenediamine, and the other raw material types, amounts and preparation methods are the same as those in the first embodiment.
[0083] Comparative Example 1
[0084] This comparative example provides a copolyamide material, which differs from Example 1 only in that the types and amounts of the raw materials remain unchanged, including hexamethylenediamine, adipic acid, pentamethylenediamine and sebacic acid; the preparation method comprises: mixing hexamethylenediamine, adipic acid, pentamethylenediamine, sebacic acid and water, reacting by increasing pressure, maintaining pressure, reducing pressure, and post-polymerization to obtain the copolyamide material, and the other steps and parameters are the same as those in Example 1.
[0085] Comparative Example 2
[0086] This comparative example provides a copolyamide material, which is different from Example 1 only in that the type and amount of the raw materials remain unchanged, including PA66 salt, pentamethylenediamine and sebacic acid; the preparation method comprises: mixing PA66 salt, pentamethylenediamine, sebacic acid and water, reacting by increasing pressure, maintaining pressure, reducing pressure, and post-polymerization to obtain the copolyamide material, and the other steps and parameters are the same as those in Example 1.
[0087] Comparative Example 3
[0088] This comparative example provides a polyamide composite material, which is different from Example 1 only in that the preparation method of the polyamide composite material includes: subjecting PA66 salt and PA510 salt to pressure maintenance, pressure reduction, and post-polymerization to obtain PA66 and PA510, and then melt-mixing PA66 and PA510 at 285°C to obtain the polyamide composite material. The other steps and parameters are the same as those in Example 1.
[0089] Performance Testing
[0090] (1) Relative viscosity: Determined in accordance with GB / T 12006.1 Plastics Polyamides Part 1: Viscosity Number;
[0091] (2) Tensile strength: According to GB / T 1040.1 Determination of tensile properties of plastics
[0092] (3) Elongation at break: Determination of tensile properties of plastics in accordance with GB / T 1040.1
[0093] (4) Melting point: Determination of melting and crystallization temperature and enthalpy in accordance with GB / T 19466.3 Plastics Differential Scanning Calorimetry (DSC) Part 3;
[0094] (5) Simply supported beam impact strength: GB / T 1043.1 Determination of simply supported beam impact properties;
[0095] (6) Dimensional change rate: The sample was injection molded into 100 mm (length) × 100 mm (width) × 1 mm
[0096] For the sample (thickness), at room temperature of 23°C, the injection molded sample was placed in a brown desiccator for conditioning for 24 hours, then quickly taken out and its vertical dimension was tested as the initial data; the sample was placed in an environment of 23°C and 100% relative humidity (immersed in deionized water) for 180 days, and the vertical dimension of the test sample was quickly taken out and used as the experimental data. The dimensional change rate (L) was calculated according to formula (1):
[0097] L=[(S 1 -S 0 ) / S 0 ]×100% (1)
[0098] S 1 S is the vertical length of the sample after absorbing moisture from the environment. 0 is the initial length of the specimen in the vertical direction.
[0099] The specific test results are shown in Table 1:
[0100] Table 1
[0101]
[0102] *: Indicates that two melting points appear and the melting point of the blend cannot be determined.
[0103] As can be seen from the above table, the copolyamide material provided by the present invention uses polyamide 66 salt and long carbon chain amide salt as raw materials, introduces a long carbon chain structure into the molecular structure of polyamide 66, and controls the ratio of polyamide 66 salt and long carbon chain amide salt, so that the copolyamide has both good strength and toughness. As can be seen from Examples 1 to 14, the tensile strength of the copolyamide material is 51.3 to 74.9 MPa, the elongation at break is 63.0 to 119.1%, and the impact strength is 5.6 to 9.0 kJ / m 2 , melting point is 208~252℃, and dimensional change rate is 1.08~1.56%.
[0104] In summary, the copolyamide provided in the present application adopts a parallel salt-forming method, using polyamide 66 salt and long-chain amide salt as raw materials to modify polyamide 66, and by controlling the ratio of the two, the copolyamide has better toughness and dimensional stability.
[0105] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A copolyamide material, characterized in that: The raw materials of the copolyamide material include polyamide 66 salt and long carbon chain amide salt.
2. The copolyamide material according to claim 1, characterized in that: The mass ratio of the polyamide 66 salt and the long carbon chain amide salt is (0.1-9):
1.
3. The copolyamide material according to claim 1 or 2, characterized in that: The raw materials of the polyamide 66 salt include adipic acid and hexamethylenediamine.
4. The copolyamide material according to any one of claims 1 to 3, characterized in that: The raw materials of the long carbon chain amide salt include long carbon chain dibasic acid and diamine; Preferably, the number of carbon atoms in the long carbon chain dibasic acid is ≥10; Preferably, the long carbon chain dibasic acid comprises at least one of decanedioic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid or pentadecanedioic acid.
5. The copolyamide material according to claim 4, characterized in that: The diamine includes C4-C14 alkyl diamine, wherein the C4-C14 alkyl diamine does not include hexamethylenediamine; Preferably, the diamine includes at least one of butanediamine, pentamethylenediamine, heptanediamine, octanediamine, decanediamine, undecanediamine, dodecanediamine or tridecanediamine.
6. A method for preparing a copolyamide material according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: The polyamide 66 salt is reacted with the long carbon chain amide salt to obtain the copolyamide material.
7. The preparation method according to claim 6, characterized in that: The polyamide 66 salt exists in the form of a polyamide 66 salt solution; Preferably, the pH value of the polyamide 66 salt solution is 7.10-7.70, and the concentration of the polyamide 66 salt solution is 50-65%; Preferably, the long carbon chain amide salt exists in the form of a long carbon chain amide salt liquid; Preferably, the pH value of the long-chain amide salt solution is 8.00-8.80, and the concentration of the long-chain amide salt solution is 60-70%; Preferably, the reaction comprises a pressure increasing stage, a pressure maintaining stage, a pressure reducing stage and a post-polymerization stage which are carried out in sequence; Preferably, the duration of the boost phase is 20 to 40 minutes; Preferably, the pressure in the pressure holding stage is 1.4-1.8 MPa; Preferably, the initial temperature of the pressure holding stage is 200-250° C., and the time of the pressure holding stage is 1-3 hours.
8. The preparation method according to claim 7, characterized in that: The depressurization stage lasts for 40 to 80 minutes, and the pressure drops to -0.002 to -0.03 MPa; Preferably, the pressure in the post-polymerization stage is -0.005 to -0.02 MPa; Preferably, the temperature of the post-polymerization stage is 230-270°C; Preferably, the post-polymerization stage lasts for 20 to 40 minutes.
9. The preparation method according to any one of claims 6 to 8, characterized in that: The preparation method comprises: The polyamide 66 salt solution and the long carbon chain amide salt solution are introduced into a closed reactor, and the pressure in the reactor is increased to 1.4-1.8MPa and the temperature is increased to 200-250°C within 20-40min, and the pressure is maintained for 1-3h, and then the pressure is reduced to -0.002-0.03MPa within 40-80min, and then the post-polymerization stage is entered, and the reaction is carried out for 20-40min under the conditions of pressure of -0.005-0.02MPa and temperature of 230-270°C to obtain the copolyamide material.
10. A modified base material, characterized in that: The modified base material comprises the copolyamide material as claimed in any one of claims 1 to 5.
Citation Information
Patent Citations
Polyamide resin composition with excellent color tone
CN104136541A
Polyamide material used for selective laser sintering and preparation method of same
CN107286338A
Synthesis method of polyamide with narrow molecular weight distribution
CN114085375A
Copolyamide resin, fiber and preparation method and application thereof
CN115536838A
Cited By
Aliphatic long-carbon-chain copolyamide resin containing oxamide component and preparation method of aliphatic long-carbon-chain copolyamide resin
CN119264415A