Method for improving thermal performance of bismaleimide resin

2,2'-diallylbisphenol A dipropargyl ether synthesized through propargyl etherification reaction and prepolymerized with bismaleimidodiphenylmethane solve the problem of insufficient mechanical properties of traditional resins at high temperatures solve the problem, achieve high heat resistance and excellent mechanical properties of the modified resin, and reduce production costs.

CN118725299APending Publication Date: 2024-10-01EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410920248.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional bismaleimide resin is difficult to maintain sufficient mechanical properties at higher temperatures, and the addition of DABPA reduces the cross-linking density of the cured resin, affecting its heat resistance.

Method used

2,2'-Diallylbisphenol A dipropargyl ether (BAPPP) was synthesized by propargyl etherification reaction between 2,2'-diallylbisphenol A and 3-halogenated propyne, and 4,4'-Bismaleimidodiphenylmethane is prepolymerized in a molten state and subsequently cured by heating to prepare a modified bismaleimide resin to improve its thermal properties.

Benefits of technology

The heat resistance and mechanical properties of bismaleimide resin are significantly improved. The glass transition temperature of the cured resin exceeds 390°C, the impact strength is greater than 6kJ m-2, the bending strength can reach more than 84MPa, and the production cost is low. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725299A_ABST
    Figure CN118725299A_ABST
Patent Text Reader

Abstract

The invention relates to a method for improving the thermal performance of bismaleimide resin. The preparation method comprises the following steps: preparing a 2, 2 '-diallyl bisphenol A dipropargyl ether compound BAPPP, pre-polymerizing 4, 4'-bismaleimidodiphenylmethane BDM and a modifier BAPPP to obtain modified maleimide resin which has good solubility and melt processability, and preparing a cured bismaleimide resin with improved thermal performance through a thermocuring process. The heat stability of the cured resin is superior to that of traditional diphenylmethane bismaleimide resin, the 5% thermal weight loss temperature of the cured resin in nitrogen is higher than 430 DEG C, the glass transition temperature of the cured resin is higher than 390 DEG C, the impact strength of the cured resin is larger than 6 kJ m <-2 >, the bending strength of the cured resin can reach 84 MPa or above, and the cured resin is an ideal matrix for preparing a high-temperature-resistant resin-based composite material and can be used for preparing the high-temperature-resistant resin-based composite material. The method has great application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-performance thermosetting resins, and in particular relates to a method for improving the thermal properties of a bismaleimide resin with excellent heat resistance. Background Art

[0002] Bismaleimide (BMI) resin, referred to as BMI resin, is a kind of high-performance thermosetting resin with wide applications. It can be used to prepare high-performance composite materials, friction materials, high-temperature resistant adhesives, high-temperature resistant insulation materials, etc., especially for the preparation of resin-based composite structural parts required for aerospace. The most widely used BMI resin is prepared by blending the bismaleimide monomer 4,4'-bismaleimide diphenylmethane (BDM) and 2,2'-diallyl bisphenol A (DABPA). This BMI resin was introduced as Ciba-Geigy's Matrimid 5292 (XU 292) resin in the 1980s. Subsequently, the QY8911 series and the "CYCOM 5250" series were launched in the domestic and foreign markets. During the melt blending of DABPA and bismaleimide, the maleimide group can undergo addition reaction with the allyl group and finally form a homogeneous system. The addition of DABPA significantly improves the processability of BDM resin and the mechanical properties of the resin cured product, making this bismaleimide resin a high-performance thermosetting resin with excellent comprehensive properties. It has been widely used in fields such as aerospace.

[0003] Due to the successful application of 2,2'-diallyl bisphenol A modified bismaleimide resin, most of the modification research on bismaleimide resin is carried out around the preparation of allyl modifiers, mainly fossil fuel-based and bio-based polyphenols are used for toughening modification of bismaleimide resin after allylation, and attempts are made to functionalize bismaleimide resin by introducing special functional groups. A modified bismaleimide resin is obtained by copolymerization of allyl ether naphthol (ANPF) and BDM. The glass transition temperature (T) of the resin prepolymerized at 140℃ for 30min and cured at 140℃~260℃ for 14h is 240℃~260℃. g ) reached 311°C, which is 44°C higher than the original resin. The quartz fiber composite material prepared with this resin as the matrix has excellent mechanical properties at 200°C (J.Appl.Polym.Sci.,2024.). A polyaryletherketone resin (RPEK-C) containing allyl group synthesized with DABPA as raw material was blended with BDM / DABPA resin system to prepare a homogeneous resin. The impact strength of the cured resin reached 10.9 kJ m -2 , than the original resin (4kJ m -2) increased by 172.5% (J.Appl.Polym.Sci.,2024,10.1002 / app.55754). An allyl functionalized cyclotriphosphazene derivative (HMACP) prepared by nucleophilic substitution of allyl methyl alcohol and eugenol was used to modify the BDM / DABPA resin system. The toughness and flame retardancy of the modified bismaleimide resin obtained by curing at 150℃~240℃ / 10h were significantly improved (Chem.Eng.J,2021,425:130655).

[0004] As a high-performance thermosetting resin, BMA resin has excellent heat resistance, and the use temperature of traditional BMA resin can exceed 200℃. However, the addition of DABPA increases the distance between the polar groups of BMA resin and reduces the crosslinking density of the cured resin. Although the toughness of the resin can be improved, the heat resistance is significantly reduced compared with pure BMA resin. Therefore, it is necessary to seek a substitute for DABPA to improve the heat resistance of the resin while maintaining the mechanical properties of the resin. BMA resin modified by alkynyl compounds has received increasing attention in recent years. Studies have shown that propargyl compounds can undergo addition reactions with maleimide groups. Similar to allyl compounds, this reaction can form a crosslinked network, and no small molecules are released during the reaction. The glass transition temperature of propargyl-terminated resin (PTR) can reach above 300℃, and it also has excellent thermal stability and low hygroscopicity. This is because propargyl groups may undergo multiple cyclization reactions during the polymerization process to form a compact and stable crosslinked structure. Blending PTR with BMA resin can improve the thermal properties of BMA resin and maintain mechanical properties. The modified bismaleimide resin (BTP) can be prepared by melt prepolymerization of polypropargyl compound (TPDDM) used to prepare polytriazole (PTA) resin and BDM. The temperature (T d5 ) and the residual rate at 800℃ (Y r800 ) reached 412℃ and 56.3%, T g Above 370°C, the flexural strength can still reach 94% of that at room temperature after being placed at 300°C for 30 minutes (React. Funct. Polym., 2023, 193: 105740.).

[0005] In order to comprehensively consider the thermal and mechanical properties of modified bismaleimide resin, the ideas of modifying bismaleimide resin with allyl compounds and propargyl compounds can be combined. At the same time, in practical applications, the extensiveness and economy of the raw material source must also be considered. After adding 4,4'-diphenyl ether dipropargyl ether (DPEDPE) to the DABPA modified BDM resin system, the T g Above 380℃, T d5It can reach 443°C (High Perform.Polym., 2021, 33:1192.); T300 carbon fiber cloth reinforced DPEDPE modified BDM / DABPA resin system composite material retains 90% and 82% of the bending strength and interlaminar shear strength at 250°C respectively compared with room temperature (Composites Science and Engineering, 2023, 11:90.). Bio-based diallyldiphenol-honokiol (honokiol, 3',5-di-2-propenyl-1,1'-biphenyl-2,4'-diphenol) is mainly derived from the dry bark, root bark and branch bark of Magnolia officinalis or Magnolia officinalis, a deciduous tree plant of the Magnoliaceae family, and is a new lignan. Honokiol propargyl ether prepared by etherification reaction of honokiol and propargyl bromide is mixed with diphenylmethane bismaleimide at 150°C for prepolymerization. The modified bismaleimide resin after curing at 150°C to 240°C for 12h has high heat resistance and mechanical properties. g Over 440℃, higher than the T of traditional DABPA modified BDM resin g (310℃), the thermal decomposition temperature is about 448℃, and the flexural strength and flexural modulus can reach 117.5MPa and 4.6GPa respectively (React.Funct.Polym.,2023,186:105570). However, honokiol is derived from natural products, and it is expensive as can be seen from Baidu search (purity ≥98%, 80.00 / 20mg (4000.00 / g), Shanghai Yuanye Biotechnology Co., Ltd.). Diallyl bisphenol A has been successfully used in modified bismaleimide resin, and its price is highly economical (purity 98%, 300.00 / kg (0.30 / g), Wuhan Kemik Biopharmaceutical Technology Co., Ltd.). Diallylphenol dipropargyl ether prepared by etherification reaction of diallyl bisphenol A (DABPA) and propargyl halide is used to modify bismaleimide resin, which has good economic efficiency. At present, there is no research report on the preparation of modified bismaleimide resin system by propargyl etherification of DABPA and copolymerization with BDM. Summary of the invention

[0006] The purpose of the present invention is to provide a method for improving the thermal properties of bismaleimide resin, so as to solve the problem that traditional bismaleimide resin is difficult to maintain sufficient mechanical properties at high temperatures. The present invention uses 2,2'-diallyl bisphenol A (DABPA) as a raw material to synthesize a bismaleimide resin modifier 2,2'-diallyl bisphenol A dipropargyl ether (BAPPP), and prepolymerizes it with 4,4'-bismaleimido diphenylmethane (BDM) in a molten state to prepare a modified bismaleimide resin, and then obtains a bismaleimide resin cured product with improved thermal properties by heating and curing, which has significantly better heat resistance than traditional bismaleimide resin.

[0007] Diallyl diphenol has been applied to the toughening modification of bismaleimide resin. These synthetic or natural diallyl diphenols can be reacted with propargyl halide (3-halopropyne) to prepare diallylphenol dipropargyl ether through Williamson etherification reaction. Due to the toughening modification of bismaleimide by allyl, and the formation of chromene structure and further crosslinking of propargyl aryl ether during thermal curing, the thermal properties of the resin system can be improved. Copolymerization of diallylphenol dipropargyl ether with bismaleimide can improve the thermal properties of bismaleimide resin and maintain or enhance the mechanical properties of bismaleimide resin. From the perspective of economy, the present invention preferably uses 2,2'-diallyl bisphenol A (DABPA) as a raw material, and reacts with propargyl halide to prepare 2,2'-diallyl bisphenol A dipropargyl ether (BAPPP) through etherification reaction.

[0008] The technical solution adopted by the present invention is:

[0009] A method for improving the thermal performance of bismaleimide resin, characterized in that the method comprises the following steps:

[0010] 1) Synthesis of modifier 2,2'-diallyl bisphenol A dipropargyl ether (BAPPP):

[0011] Route 1: Using 2,2'-diallyl bisphenol A and 3-halopropyne as raw materials, propargyl etherification is carried out by phase transfer catalysis, that is, 2,2'-diallyl bisphenol A, phase transfer catalyst, sodium hydroxide and deionized water are mixed and mechanically stirred, and the mass ratio of 2,2'-diallyl bisphenol A, phase transfer catalyst and sodium hydroxide per liter of deionized water is (150-160) g: (20-35) g: (90-120) g, 3- Halogenated propyne is dissolved in toluene and added dropwise therein, wherein the molar ratio of phenolic hydroxyl group and 3-halogenated propyne in 2,2'-diallyl bisphenol A is 1.0:(1.0-1.5), heated at 20°C-80°C, reacted at constant temperature for 4h-20h, the upper liquid is separated, and the volatile components are removed after washing, drying and rotary evaporation to obtain 2,2'-diallyl bisphenol A dipropargyl ether BAPPP; wherein the phase transfer catalyst is tetrabutylammonium bromide or benzyltriethylammonium chloride;

[0012] or,

[0013] Route 2: Using 2,2'-diallyl bisphenol A and 3-halopropyne as raw materials, propargyl etherification is carried out through Williamson etherification reaction, that is, 2,2'-diallyl bisphenol A is dissolved in an organic solvent, anhydrous potassium carbonate is added at a molar ratio of 2,2'-diallyl bisphenol A: anhydrous potassium carbonate of 1: (2-10) and mechanical stirring is performed, and then 3-halopropyne is added, and the molar ratio of phenolic hydroxyl group in 2,2'-diallyl bisphenol A to 3-halopropyne is 1.0: (1.0-1 .5), heating to 50°C to 60°C, reacting at a constant temperature for 6h to 16h, filtering and separating to remove the solvent, and then using an organic solvent immiscible with water to dissolve the filtrate, and removing the organic volatile components after washing and drying to obtain 2,2'-diallyl bisphenol A dipropargyl ether BAPPP; wherein the solvent used to dissolve 2,2'-diallyl bisphenol A is acetone or N,N'-dimethylformamide DMF, and the organic solvent immiscible with water is one selected from toluene, ethyl acetate, and dichloromethane;

[0014] In the above reaction, the general structural formula of 3-halopropyne is Wherein, X is Cl or Br;

[0015] 2) Preparation of modified bismaleimide resin prepolymer:

[0016] The molar ratio of 4,4'-bismaleimide diphenylmethane BDM: 2,2'-diallyl bisphenol A dipropargyl ether BAPPP is 1.0: (0.7-1.0) and the two components are mixed, heated to 120°C-150°C for melt prepolymerization, and stirred for 0.5h-2.0h to obtain a modified bismaleimide resin prepolymer; wherein,

[0017] The structure of 4,4'-bismaleimidodiphenylmethane is:

[0018] The structure of 2,2'-diallyl bisphenol A dipropargyl ether is:

[0019]

[0020] (3) Preparation of bismaleimide resin cured product with improved thermal properties:

[0021] The modified bismaleimide resin prepolymer obtained in step (2) is poured into a preheated mold at 80°C to 120°C, and a differential scanning calorimeter (DSC) is used to determine the stage temperature rise program for heating and curing the resin prepolymer, and heating and curing are performed to obtain a bismaleimide resin cured product with improved performance.

[0022] Preferably, in route 1 and route 2 of step (1), the molar ratio of phenolic hydroxyl group:3-halopropyne is 1.0:1.1.

[0023] Preferably, in route 1 and route 2 of step (1), the washing method is to use a saturated sodium carbonate solution or a saturated sodium bicarbonate solution to wash 2 to 3 times, and then use deionized water to wash 1 to 2 times until neutral.

[0024] Preferably, in route 1 and route 2 of step (1), the drying method is to add a desiccant and stir, and then filter and remove the desiccant after standing overnight, and the desiccant is selected from one of anhydrous sodium sulfate, sodium carbonate, potassium sulfate, potassium carbonate, magnesium sulfate, and magnesium carbonate.

[0025] Preferably, in route 1, the heating temperature is 60° C. to 80° C., and the reaction time is 12 h to 16 h.

[0026] Preferably, in route 2, the heating temperature is 55°C to 60°C, and the reaction time is 8-12h.

[0027] Preferably, in route 2, the molar ratio of 2,2'-diallylbisphenol A to anhydrous potassium carbonate is 1:5.

[0028] Preferably, in step (2), the molar ratio of 4,4'-bismaleimidodiphenylmethane BDM:2,2'-diallylbisphenol A dipropargyl ether BAPPP is 1:0.85.

[0029] Preferably, the heating curing in step (3) is carried out in an oven or a tubular furnace in an air atmosphere.

[0030] Beneficial Effects

[0031] 1. The raw materials used in the present invention are widely available and relatively cheap. Among them, 4,4'-bismaleimidodiphenylmethane (BDM) is a representative raw material for commercial bismaleimide resins; the raw material source of 2,2'-diallylbisphenol A (DABPA) is bisphenol A, which is a petrochemical product with large output, low price and wide application. 2,2'-diallylbisphenol A (DABPA) synthesized with bisphenol A as raw material is also a commercial product. The chemicals used in the synthesis process of 2,2'-diallylbisphenol A dipropargyl ether (BAPPP) are all common chemicals, and the selectable organic solvents such as toluene, acetone, DMF, ethyl acetate, etc. are all common organic solvents. Therefore, the modified bismaleimide resin prepared by blending and modifying BAPPP and BDM has obvious advantages in production cost.

[0032] 2. The method for improving the thermal properties of bismaleimide resin is simple and easy, and only involves the mixing and heating and stirring process of two components. The obtained modified bismaleimide resin is uniform and transparent, has a wide low-viscosity processing window and a long gel time, can be dissolved in common organic solvents such as acetone, tetrahydrofuran, ethyl acetate, etc., and is suitable for composite material molding processes such as molding, prepreg molding, resin transfer molding (RTM) and wet winding molding.

[0033] 3. The modified bismaleimide resin prepared in the present invention has excellent heat resistance. The 5% thermal weight loss temperature of the resin cured product in nitrogen is greater than 430°C, the glass transition temperature measured by dynamic thermodynamic analysis (DMA) is greater than 390°C, and the impact strength is greater than 6 kJ m -2 , the bending strength can reach over 84MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The infrared spectra of the allyl aryl propargyl ether monomer 2,2'-diallyl bisphenol A dipropargyl ether and the raw material 2,2'-diallyl bisphenol A synthesized in the present invention;

[0035] Figure 2 is the DSC curve of the modified bismaleimide resin prepolymer prepared in Example 3 of the present invention in nitrogen;

[0036] Figure 3 is a thermogravimetric analysis (TGA) curve of the modified bismaleimide resin cured product prepared in Example 3-5 of the present invention in nitrogen;

[0037] Figure 4 DMA curve of the modified bismaleimide resin cured product prepared in Example 3-5 of the present invention in nitrogen; DETAILED DESCRIPTION

[0038] In order to more clearly and completely illustrate the technical solution and advantages of the present invention, the technical solution adopted by the present invention is described in detail below through embodiments. The described embodiments are only for illustration and are not intended to limit the scope of protection of the present invention.

[0039] The 4,4'-bismaleimidodiphenylmethane used in the examples of the present invention was purchased from Hubei Honghu Shuangma New Material Technology Co., Ltd., and the 2,2'-diallylbisphenol A was purchased from Shanghai Huaming High-Tech Co., Ltd.

[0040] The staged temperature rise program of the thermal curing of the modified bismaleimide resin in the present invention is determined based on the exothermic curve obtained by testing the prepolymerized resin through a differential scanning calorimeter, and the specific exothermic condition is related to the ratio of the resin raw materials.

[0041] In the following examples:

[0042] The structure of the synthesized allyl aryl propargyl ether monomer 2,2'-diallyl bisphenol A dipropargyl ether was characterized using a Nicolet iS10 infrared spectrometer from Thermo Fisher, USA.

[0043] The thermal curing step-wise temperature rise program of the modified bismaleimide resin prepolymer was obtained by DSC test. The instrument used was a Q 2000 differential scanning calorimeter from TA Company of the United States. The heating rate was 10 °C min -1 , nitrogen flow rate is 50mL·min -1 .

[0044] The thermal stability of the modified bismaleimide resin cured product was tested using a thermogravimetric analyzer. The instrument used was a TGA-DSC1 thermogravimetric synchronous thermal analyzer produced by Mettler Toledo, Switzerland. The heating rate was 10°C / min and the nitrogen flow rate was 60 mL / min.

[0045] The glass transition temperature of the modified bismaleimide resin cured product was tested using a dynamic thermomechanical analyzer. The instrument used was a DMA1 dynamic thermomechanical analyzer from Mettler Toledo, Switzerland, with a heating rate of 5°C / min and a frequency of 1 Hz.

[0046] After demoulding, the modified bismaleimide resin cured product was polished to a smooth surface using an MPZ-1 metallographic polishing machine produced by Shanghai Minxin Testing Instrument Co., Ltd. The polishing machine speed was 300 rpm.

[0047] The impact performance test of the modified bismaleimide resin cured product was carried out according to the reference standard ISO-180, and the instrument used was the CEAST 9050 cantilever beam impact tester produced by CEAST Company of Italy.

[0048] The bending properties of modified bismaleimide resin cured product were tested according to the standard GB / T2567-2021, and the instrument used was Shenzhen Sansi's CMT5504 electronic universal testing machine.

[0049] Example 1

[0050] First synthesize the modifier 2,2'-diallyl bisphenol A dipropargyl ether (BAPPP)

[0051] 30.84 g of 2,2'-diallylbisphenol A (DABPA), 6.45 g of tetrabutylammonium bromide, 20 g of sodium hydroxide and 200 mL of deionized water were added in sequence into a 500 mL four-necked round-bottom flask. DABPA was completely dissolved by mechanical stirring. 26.17 g of 3-bromopropyne was dissolved in toluene and added dropwise to the system. The temperature was raised to 80°C and kept constant for 12 h.

[0052] After the reaction is completed, the upper oil phase is taken and washed with saturated sodium carbonate solution and deionized water to neutrality. After adding anhydrous sodium sulfate to remove the remaining water, the solvent is removed by rotary evaporation and the residual volatiles are removed in a vacuum oven at 100°C for 1 hour to obtain a dark yellow liquid, which is 2,2'-diallyl bisphenol A dipropargyl ether (BAPPP).

[0053] or:

[0054] Dissolve 30.84 g of 2,2'-diallylbisphenol A (DABPA) in 300 mL of acetone and add into a 500 mL four-necked round-bottom flask. Then add 69.10 g of anhydrous potassium carbonate. After mechanical stirring for 1 h, add 16.38 g of 3-chloropropyne and heat to 58 °C for 10 h.

[0055] After the reaction, the solvent was removed by rotary evaporation, and the residue was dissolved in 150 mL of ethyl acetate. The solution was washed with saturated sodium carbonate solution and deionized water until neutral. After adding anhydrous sodium sulfate to remove the remaining water, the solvent was removed by rotary evaporation and the residual volatiles were removed in a vacuum oven at 100°C for 1 hour to obtain a dark yellow liquid, which was 2,2'-diallyl bisphenol A dipropargyl ether (BAPPP).

[0056] Add 57.10 g of 4,4'-bismaleimide diphenylmethane and 42.90 g of 2,2'-diallyl bisphenol A dipropargyl ether into a 250 mL four-necked round-bottom flask, heat to 130°C and start stirring at a stirring speed of 180 rpm for 0.5 h to obtain a dark yellow homogeneous liquid, which is a modified bismaleimide resin prepolymer.

[0057] The resin was poured into a preheated mold with a release agent on the surface while still hot, placed in a vacuum oven, heated to 100°C, and vacuum degassed at a pressure of -0.1 MPa for 1 hour.

[0058] After the resin was vacuum degassed, the staged temperature rise curing process of BAPPP and BDM prepolymer resin was determined by differential scanning calorimetry. The DSC curves obtained by the test (see Figure 3) shows that the resin curing reaction temperature determines that the staged temperature-rising curing program of the modified bismaleimide resin is: 130℃ / 2h+150℃ / 1h+180℃ / 1h+200℃ / 2h+230℃ / 2h. The cured resin was subjected to DSC analysis, and no resin curing exothermic peak was observed, indicating that the resin can be completely cured according to this curing process.

[0059] The resin in the mold is heated and cured in an oven at a process of 130℃ / 2h+150℃ / 1h+180℃ / 1h+200℃ / 2h+230℃ / 2h, and then slowly cooled to room temperature in the oven. After the solidified material is demolded, the surface is polished with a metallographic polisher until it is smooth and flat.

[0060] The performance test results of the modified bismaleimide resin cured product obtained in Example 1 are shown in Table 1.

[0061] Example 2

[0062] The synthesis of the modifier 2,2'-diallyl bisphenol A dipropargyl ether (BAPPP) is as in Example 1.

[0063] Add 52.31 g of 4,4'-bismaleimide diphenylmethane and 47.69 g of 2,2'-diallyl bisphenol A dipropargyl ether into a 250 mL four-necked round-bottom flask, heat to 130°C and start stirring at a stirring speed of 180 rpm for 0.5 h to obtain a dark yellow homogeneous liquid, which is a modified bismaleimide resin prepolymer.

[0064] The resin was poured into a preheated mold and an aluminum box with a release agent on the surface while hot, placed in a vacuum oven, heated to 100°C, and vacuum degassed at a pressure of -0.1 MPa for 1 hour.

[0065] After the resin was vacuum degassed, the staged temperature-rising curing program of the modified bismaleimide resin was determined by differential scanning calorimetry. The DSC curve obtained from the test showed that the staged temperature-rising curing program of the modified bismaleimide resin was: 130°C / 2h+150°C / 1h+180°C / 1h+200°C / 2h+230°C / 2h. The cured resin was subjected to DSC analysis, and no exothermic peak of resin curing was observed, indicating that the resin can be completely cured according to this curing process.

[0066] The resin in the mold is heated and cured in an oven at a process of 130℃ / 2h+150℃ / 1h+180℃ / 1h+200℃ / 2h+230℃ / 2h, and then slowly cooled to room temperature in the oven. After the solidified material is demolded, the surface is polished with a metallographic polisher until it is smooth and flat.

[0067] The performance test results of the modified bismaleimide resin cured product obtained in Example 2 are shown in Table 1.

[0068] Example 3

[0069] The synthesis of the modifier 2,2'-diallyl bisphenol A dipropargyl ether (BAPPP) is as in Example 1.

[0070] Add 48.20 g of 4,4'-bismaleimide diphenylmethane and 51.80 g of 2,2'-diallyl bisphenol A dipropargyl ether into a 250 mL four-necked round-bottom flask, heat to 130°C and start stirring at a stirring speed of 180 rpm for 0.5 h to obtain a dark yellow homogeneous liquid, which is a modified bismaleimide resin prepolymer.

[0071] The resin was poured into a preheated mold and an aluminum box with a release agent on the surface while hot, placed in a vacuum oven, heated to 100°C, and vacuum degassed at a pressure of -0.1 MPa for 1 hour.

[0072] After the resin was vacuum degassed, the staged temperature-rising curing program of the modified bismaleimide resin was determined by differential scanning calorimetry. The resin curing reaction temperature shown by the DSC curve obtained from the test determined that the staged temperature-rising curing program of the modified bismaleimide resin was: 130°C / 2h+150°C / 1h+180°C / 1h+200°C / 2h+230°C / 2h. The cured resin was subjected to DSC analysis, and no resin curing exothermic peak was observed, indicating that the resin can be completely cured according to this curing process.

[0073] The resin in the mold is heated and cured in an oven at a process of 130℃ / 2h+150℃ / 1h+180℃ / 1h+200℃ / 2h+230℃ / 2h, and then slowly cooled to room temperature in the oven. After the solidified material is demolded, the surface is polished with a metallographic polisher until it is smooth and flat.

[0074] The performance test results of the modified bismaleimide resin cured product obtained in Example 3 are shown in Table 1.

[0075] Table 1 Performance test results of the modified bismaleimide resin cured products in Examples 3-5.

[0076]

[0077]

[0078] The data in Table 1 show that the impact strength of the modified bismaleimide resin cured product obtained in Examples 1-3 decreases with the increase of the content of 4,4'-diallyl bisphenol A dipropargyl ether in the resin as component B, the flexural strength is less affected by the change of the content of component B, and the flexural modulus increases with the increase of the content of component B; the modified bismaleimide resin cured product obtained in Examples 3-5 has excellent heat resistance, and its thermal stability and glass transition temperature are little affected by the change of the content of component B, showing the potential of the modified bismaleimide resin cured product for application in an environment with a temperature above 300°C.

[0079] The modified bismaleimide resin of BAPPP modified BDM is suitable for various composite material molding methods such as hand lay-up molding, prepreg automatic placement molding, resin transfer molding (RTM) molding and wet winding molding, and has great application potential in the preparation of high-temperature resistant structural parts and other composite materials products.

Claims

1. A method for improving the thermal properties of bismaleimide resin, It is characterized in that The method comprises the following steps: (1) Synthesis of modifier 2,2'-diallyl bisphenol A dipropargyl ether (BAPPP): Route 1: Using 2,2'-diallyl bisphenol A and 3-halopropyne as raw materials, propargyl etherification is carried out by phase transfer catalysis, that is, 2,2'-diallyl bisphenol A, phase transfer catalyst, sodium hydroxide and deionized water are mixed and mechanically stirred, and the mass ratio of 2,2'-diallyl bisphenol A, phase transfer catalyst and sodium hydroxide per liter of deionized water is (150-160) g: (20-35) g: (90-120) g, 3-halopropyne is Dissolve propyne in toluene and dropwise add the molar ratio of phenolic hydroxyl group and 3-halogenated propyne in 2,2'-diallyl bisphenol A to 1.0:(1.0-1.5), heat at 20°C-80°C, react at constant temperature for 4h-20h, separate the upper liquid, wash, dry, and remove volatile components by rotary evaporation to obtain 2,2'-diallyl bisphenol A dipropargyl ether BAPPP; wherein the phase transfer catalyst is tetrabutylammonium bromide or benzyltriethylammonium chloride; or, Route 2: Using 2,2'-diallyl bisphenol A and 3-halopropyne as raw materials, propargyl etherification is carried out through Williamson etherification reaction, that is, 2,2'-diallyl bisphenol A is dissolved in an organic solvent, anhydrous potassium carbonate is added at a molar ratio of 2,2'-diallyl bisphenol A: anhydrous potassium carbonate of 1: (2-10) and mechanical stirring is performed, and then 3-halopropyne is added, and the molar ratio of phenolic hydroxyl group in 2,2'-diallyl bisphenol A to 3-halopropyne is 1.0: (1.0-1 .5), heating to 50°C to 60°C, reacting at a constant temperature for 6h to 16h, filtering and separating to remove the solvent, and then using an organic solvent immiscible with water to dissolve the filtrate, and removing the organic volatile components after washing and drying to obtain 2,2'-diallyl bisphenol A dipropargyl ether BAPPP; wherein the solvent used to dissolve 2,2'-diallyl bisphenol A is acetone or N,N'-dimethylformamide DMF, and the organic solvent immiscible with water is one selected from toluene, ethyl acetate, and dichloromethane; In the above reaction, the general structural formula of 3-halopropyne is Wherein, X is Cl or Br; (2) Preparation of modified bismaleimide resin prepolymer: The molar ratio of 4,4'-bismaleimide diphenylmethane BDM: 2,2'-diallyl bisphenol A dipropargyl ether BAPPP is 1.0: (0.7-1.0) and the two components are mixed, heated to 120°C-150°C for melt prepolymerization, and stirred for 0.5h-2.0h to obtain a modified bismaleimide resin prepolymer; wherein, The structure of 4,4'-bismaleimidodiphenylmethane is: The structure of 2,2'-diallyl bisphenol A dipropargyl ether is: (3) Preparation of bismaleimide resin cured product with improved thermal properties: The modified bismaleimide resin prepolymer obtained in step (2) is poured into a preheated mold at 80°C to 120°C, and a differential scanning calorimeter (DSC) is used to determine the stage temperature rise program for heating and curing the resin prepolymer, and heating and curing are performed to obtain a bismaleimide resin cured product with improved thermal properties.

2. The method for improving the thermal properties of bismaleimide resin according to claim 1, It is characterized in that In route 1 and route 2 of step (1), the molar ratio of phenolic hydroxyl group to 3-halopropyne is 1.0:1.

1.

3. The method for improving the thermal properties of bismaleimide resin as claimed in claim 1, It is characterized in that In route 1 and route 2 of step (1), the washing method is to use a saturated sodium carbonate solution or a saturated sodium bicarbonate solution to wash 2 to 3 times, and then use deionized water to wash 1 to 2 times until neutral.

4. The method for improving the thermal properties of bismaleimide resin according to claim 1, It is characterized in that In route 1 and route 2 of step (1), the drying method is to add a desiccant and stir, and then filter and remove the desiccant after standing overnight. The desiccant is selected from one of anhydrous sodium sulfate, sodium carbonate, potassium sulfate, potassium carbonate, magnesium sulfate, and magnesium carbonate.

5. The method for improving the thermal properties of bismaleimide resin according to claim 1, It is characterized in that In the first route, the heating temperature is 60° C. to 80° C., and the reaction time is 12 h to 16 h.

6. The method for improving the thermal properties of bismaleimide resin according to claim 1, It is characterized in that In the second route, the heating temperature is 55°C to 60°C, and the reaction time is 8h to 12h.

7. The method for improving the thermal properties of bismaleimide resin according to claim 1, It is characterized in that In the second route, the molar ratio of 2,2'-diallyl bisphenol A to anhydrous potassium carbonate is 1:

5.

8. The method for improving the thermal properties of bismaleimide resin according to claim 1, It is characterized in that In the step (2), the molar ratio of 4,4'-bismaleimidodiphenylmethane BDM to 2,2'-diallylbisphenol A dipropargyl ether BAPPP is 1:0.

85.

9. The method for improving the thermal properties of bismaleimide resin according to claim 1, It is characterized in that The heating and curing in step (3) is carried out in an oven or a tubular furnace in an air atmosphere.