Bonding and lubricating double-sided double-strand-chain high-entanglement polyelectrolyte compound hydrogel as well as preparation method and application thereof

By adopting a double-layer structure design in the polymer hydrogel, combined with multiple hydrogen bonds and electrostatic interactions, the problem of high adhesion and high lubricity in the existing technology is solved, and high toughness and water swelling resistance are achieved. Double-layer hydrogel, a substitute material for artificial biological tissues.

CN118725344APending Publication Date: 2024-10-01HUBEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410712479.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult for existing polymer hydrogels to simultaneously achieve high adhesion and high lubrication properties when used in biological tissues, and it is difficult to balance toughness and water swelling resistance, resulting in limited applications in biological tissues.

Method used

A double-layer hydrogel preparation method is adopted, by mixing chitosan quaternary ammonium salt and hyaluronic acid powder, adding cross-linking agents and initiators, and performing annealing and polymerization cross-linking to form multiple hydrogen bond physical cross-links. The double-stranded chain structure, combined with electrostatic interaction, prepares a double-layer hydrogel with high adhesion on one side and high lubrication on the other.

Benefits of technology

It achieves the high toughness, good tensile strength and water swelling resistance of the hydrogel, and also has excellent adhesion properties and lubricity, making it suitable as a substitute material for artificial biological tissues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725344A_ABST
    Figure CN118725344A_ABST
Patent Text Reader

Abstract

The invention relates to a bonding lubrication double-sided double-strand-chain high-entanglement polyelectrolyte compound hydrogel and a preparation method and application thereof, cation HACC and anion HA are homogenized through kneading and annealing, the cation HACC and the anion HA are converted into a tightly-entangled double-strand-chain structure through electrostatic interaction between molecular chains, an HACC / HA layer structure is fixed through a small number of covalent bonds, and high lubricity is achieved; a highly entangled TA-coated HACC / HA layer is obtained by directly kneading a multi-hydrogen-bond physical crosslinking double-strand chain structure through TA, the TA-coated HACC / HA layer has almost perfect elasticity, high tensile strength, high toughness and high adhesion, a double-layer hydrogel structure is obtained through mold pressing and illumination, and the TA-coated HACC / HA hydrogel can be used for rapidly adhering and repairing potential materials for tissue wounds in organisms and preventing back tissue adhesion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a "adhesive-lubricating double-sided" double-stranded chain highly entangled polyelectrolyte complex hydrogel and a preparation method and application thereof. Background Art

[0002] Surgical adhesive tape is used to quickly bond and repair wounds on biological internal tissues. The adhesive tape will quickly bond with the tissues within a few seconds, and at the same time, it is also necessary to separate different parts of tissues and organs from each other, showing the characteristics of high adhesion on one side and high lubricity on the other side. At the same time, the adhesive tape can expand and contract with the functioning organs during the wound healing process and maintain for a period of time. Once the injury is completely healed, the adhesive tape will gradually degrade without causing adhesion to the surrounding tissues and causing inflammation.

[0003] Polysaccharide hydrogels have high water content and high tissue compatibility, and are potential substitutes for artificial biological tissues. Synthetic hydrogels are generally obtained by polymerizing and crosslinking hydrophilic monomers in water, and natural hydrogels are generally obtained by crosslinking hydrophilic natural polymers in water. However, these methods are limited by the fact that hydrophilic monomers or hydrophilic natural polymers have only a certain solubility in water, and the polymer hydrogels obtained have low polymer content. CN117402377A discloses a high compression strength cellulose hydrogel that utilizes the synergistic effect of salting-out effect and ion coordination, which has a certain anti-swelling performance, but the elongation at break is less than 80%. CN113754903A discloses a polysaccharide hydrogel cross-linked by ultraviolet light without initiator, which has poor toughness (0.2-0.7MPa, 40-70%). In this way, water swelling resistance is obtained by increasing the degree of cross-linking, but the toughness is low. On the contrary, the toughness is increased by reducing the degree of cross-linking, but the water swelling resistance is poor. The interaction between polyelectrolyte molecules and water molecules is much higher than that of general hydrophilic polymers. It is more difficult to obtain strong toughness and water swelling resistance through ordinary cross-linked polyelectrolyte hydrogels. CN117414464A obtains a polysaccharide hydrogel dressing with unilateral adhesion ability Janus by coating a polymer brush layer on one side of a zwitterionic hydrogel and cross-linking it by ultraviolet light. The gel easily absorbs water and swells. On the other hand, polyelectrolyte polysaccharides play an important role in biological tissues. Many biological tissues in nature form stable molecular structures and functions through double strands. Summary of the invention

[0004] The invention aims to provide a double-layer hydrogel with a smooth surface layer and a highly bonded bottom layer and a preparation method thereof.

[0005] The solution adopted by the present invention to solve the above technical problems is:

[0006] A method for preparing a "adhesive-lubricating double-sided" double-stranded chain highly entangled polyelectrolyte complex hydrogel comprises the following steps:

[0007] (1) chitosan quaternary ammonium salt (HACC), hyaluronic acid powder (HA), a cross-linking agent, an initiator, and water are uniformly mixed to obtain a dough-like HACC / HA composite polysaccharide, wherein the molar ratio of the repeating units of chitosan quaternary ammonium salt to hyaluronic acid is 1:0.7-1.3;

[0008] (2) chitosan quaternary ammonium salt, hyaluronic acid powder, tannic acid (TA), and water are uniformly mixed to obtain a dough-like TA@HACC / HA composite polysaccharide, wherein the molar ratio of the repeating units of chitosan quaternary ammonium salt to hyaluronic acid is 1:0.7-1.3;

[0009] (3) allowing the composite polysaccharide dough obtained in step (1) and step (2) to stand and relax, and then shaping the dough to obtain a sheet-like HACC / HA precursor sheet and a TA@HACC / HA precursor sheet;

[0010] (4) annealing the obtained precursor sheet to obtain preformed HACC / HA hydrogel and TA@HACC / HA hydrogel;

[0011] (5) The preformed HACC / HA hydrogel and TA@HACC / HA hydrogel are laminated to initiate polymerization and cross-linking to obtain a highly entangled TA@HACC / HA and HACC / HA double-layer hydrogel with a double-stranded chain structure physically cross-linked by multiple hydrogen bonds.

[0012] Preferably, the HACC and HA in step (1) are both in powder form, which is convenient for rapid absorption of solvent, swelling and dissolution.

[0013] Preferably, in the composite polysaccharide powder obtained in step (1), the molar ratio of the repeating units of HACC and HA is 1:0.7-1.3, for example, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3.

[0014] Preferably, in the HACC / HA composite polysaccharide and TA@HACC / HA composite polysaccharide obtained in step (1) and step (2), the total molar concentration of the repeating units of HACC and HA is 1.1-2.8 mol / L, such as 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L, 2.0 mol / L, 2.1 mol / L, 2.2 mol / L, 2.3 mol / L, 2.4 mol / L, 2.5 mol / L, 2.6 mol / L, 2.7 mol / L, 2.8 mol / L. The natural polysaccharide polymer powders of opposite charges are uniformly mixed in a small amount of solvent to form a dough-like precursor material, which can be plastically treated and has a certain shape retention ability. Subsequent treatment can fix the shape of the hydrogel product and further improve the mechanical strength of the hydrogel, showing good processing performance.

[0015] Preferably, in the dough-like TA@HACC / HA composite polysaccharide obtained in step (2), the content of TA is 8% to 14% of the total mass of the composite polysaccharide powder, for example 8%, 10%, 12%, 14%. In the process of preparing the dough-like composite polysaccharide, TA physically cross-links the double-stranded chain structure through multiple hydrogen bonds to obtain a highly entangled hydrogel. The mechanism of action of the two is as shown in the attached Figure 1 shown.

[0016] Preferably, the crosslinking agent is glycerol methacrylate (GMA), and the initiator is α-ketoglutaric acid (KA).

[0017] Preferably, the ratio of the molar concentration of the cross-linking agent to the total molar concentration of the repeating units of HACC and HA is (0.004-0.008):1, for example, 0.004:1, 0.006:1, 0.008:1; the ratio of the molar concentration of the initiator to the molar concentration of GMA is (0.15-0.25):1, for example, 0.15:1, 0.2:1, 0.25:1.

[0018] Preferably, the mixing method in step (1) and step (2) is not particularly limited, such as mechanical stirring, kneading, rubbing, beating, repeated molding-folding-molding or a combination thereof. The purpose of mixing is to make the HACC molecular chains containing cations and the HA molecular chains containing anions fully contact to generate electrostatic interaction, and then transform into a tightly wound double-stranded chain structure, and the TA multi-hydrogen bond physical cross-linking double-stranded chain structure to obtain a highly entangled hydrogel structure. The degree of mixing is preferably to obtain a transparent homogeneous dough-like precursor.

[0019] Preferably, in step (3), the composite polysaccharide dough is left to stand for a period of time similar to "proofing", so that the internal stress between the molecular chains is gradually released during the process, so that the distribution of the entangled double-stranded chain structure reaches a balance. The treatment temperature is 10-40° C. and the time is 0.1-3 hours.

[0020] Preferably, the method of shaping the composite polysaccharide dough in step (3) is molding.

[0021] Preferably, in step (3), the composite polysaccharide dough is repeatedly subjected to a molding-folding-molding process during the molding process.

[0022] Preferably, the thickness of the HACC / HA precursor sheet and the TA@HACC / HA precursor sheet obtained in step (3) is 0.1 to 3 mm.

[0023] Preferably, the annealing treatment in step (4) is carried out under constant temperature and humidity conditions, the annealing temperature is 50-60° C., the time is 12-24 hours; the ambient humidity is 90%-100%, more preferably 98%.

[0024] The present invention also provides a "adhesive-lubricating double-sided" double-stranded chain highly entangled polyelectrolyte complex hydrogel, which is prepared by the above method.

[0025] The present invention also provides the application of the above-mentioned "adhesive-lubricating double-sided" double-stranded chain highly entangled polyelectrolyte complex hydrogel for preparing artificial biological tissue substitute materials.

[0026] The present invention produces a tough, swelling-resistant, high-polymer-content polysaccharide-polyelectrolyte complex hydrogel by simply kneading and annealing the composite polysaccharide-polyelectrolyte (cationic HACC and anionic HA) dough. The dough is homogenized by kneading and annealing, and converted into a tightly wound double-stranded chain structure by utilizing the electrostatic interaction between molecular chains; the addition of TA further brings about multiple hydrogen bond physical crosslinking to obtain a highly entangled TA@HACC / HA layer hydrogel with nearly perfect elasticity, high tensile strength, and high toughness. The HACC / HA physical crosslinked double-stranded chain structure is fixed by a small amount of covalent bonds to obtain a HACC / HA hydrogel. The two layers of hydrogel are bonded together to initiate the polymerization and crosslinking of the HACC / HA hydrogel to obtain a double-layer gel with high adhesion on one side (TA@HACC / HA) and high lubricity on the other side (HACC / HA).

[0027] At the same time, both positively and negatively charged polyampholyte hydrogels have self-adjusting adhesive properties. Through the charge rearrangement of the double electric layer, the hydrogel will adhere to the electrostatic biological tissue at the interface through the mutual attraction of positive and negative opposite charges. In addition, the multiple hydrogen bonds of TA and the electrostatic adhesion of polyampholytes work together to make the hydrogel have excellent adhesion properties to the biological tissue. On the other hand, the hydrogel has an extremely high ionic group density to the outer layer HACC / HA complex polysaccharide polyelectrolyte, and the hydration free energy of the zwitterionic group (about -200 to -300 kJ / mol) is lower than that of the non-ionic hydrophilic polymer (about -100 to -200 kJ / mol), and has stronger affinity and hydrophilicity with water. Therefore, it is very easy to form a dense hydration layer on the surface of the gel, so that the hydrogel adhesive tape has good lubricity to the outer layer HACC / HA.

[0028] Compared with the prior art, the present invention has the following advantages and significant progress:

[0029] The present invention utilizes a very small amount of aqueous solution environment to convert the electrostatic interaction between chitosan quaternary ammonium salt and hyaluronic acid molecular chains into a tightly wound double-stranded chain structure, and utilizes tannic acid multiple hydrogen bonds to physically cross-link the double-stranded chain structure to obtain highly entangled TA@HACC / HA, which has nearly perfect elasticity, high tensile strength, and high toughness, and has excellent adhesion performance with biological tissues through electrostatic interaction and synergistic effects enhanced by multiple hydrogen bonds; on the other hand, a HACC / HA layer hydrogel network is obtained by fixing the double-stranded chain structure with a small amount of covalent bonds, and a dense hydration layer is formed on the surface of the HACC / HA gel, so that the hydrogel adhesive tape has good lubricity, can avoid adhesion to tissues, and can be used as a potential substitute material for artificial biological tissues. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The present invention is further described with reference to the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention.

[0031] Figure 1 It is a schematic diagram of the design process of TA@HACC / SA and HACC / SA double-layer hydrogel of the present invention;

[0032] Figure 2 This is a mechanism diagram of the present invention using TA multi-hydrogen bonds to physically cross-link the double-stranded chain structure;

[0033] Figure 3 is a comparison chart of the anti-swelling properties of the hydrogels obtained in Examples 1 to 3 and Comparative Examples 3 to 5;

[0034] Figure 4 is a comparison chart of the mechanical properties of the hydrogels obtained in Examples 1 to 3 and Comparative Examples 2 to 5;

[0035] Figure 5 is a comparison chart of the adhesive properties of the hydrogels obtained in Examples 1 to 3 and Comparative Examples 2 to 5;

[0036] Figure 6 It is the interface toughness between the adhesive layer and the lubricating layer of the double-layer hydrogel obtained in Examples 1 to 3. DETAILED DESCRIPTION

[0037] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0038] Example 1

[0039] Step (1): Weigh HACC powder and HA powder and mix them evenly in a round-bottom evaporating dish to obtain a uniform composite polysaccharide powder having a repeating unit molar ratio of HACC to HA of 1:1, in total two portions.

[0040] Step (2): Add 8 wt% TA and a small amount of water to one of the composite polysaccharide powders, so that the total molar concentration of HACC and HA repeating units in the mixture is 2.8 mol / L, and knead to obtain TA@HACC / HA composite polysaccharide dough. Add a small amount of GMA (the ratio of the total molar concentration of HACC and HA repeating units is 0.004:1) and a small amount of KA (the ratio of the total molar concentration of HACC and HA repeating units is 0.15:1) and a small amount of water to the other composite polysaccharide powder, so that the total molar concentration of HACC and HA repeating units in the mixture is 2.8 mol / L, and knead to obtain HACC / HAC composite dough.

[0041] Step (3): After the two composite polysaccharide doughs are placed at room temperature (25° C.) for 2 hours, they are repeatedly molded-folded-molded three times using a mold consisting of a 0.3 mm PET rectangular frame and a pair of glass plates at room temperature to obtain a transparent and homogeneous precursor sheet.

[0042] Step (4): The obtained precursor sheet was placed in a constant temperature and humidity chamber at 50° C. for annealing for 24 hours to obtain a preformed HACC / HA hydrogel and a preformed TA@HACC / HA hydrogel.

[0043] Step (5): The obtained preformed HACC / HA hydrogel and preformed TA@HACC / HA hydrogel are laminated and molded for 20 minutes, and the HACC / HA surface is exposed to ultraviolet light for 1 hour to achieve sufficient covalent crosslinking, thereby obtaining a multi-hydrogen bond physically crosslinked double-stranded chain structure to obtain a highly entangled HACC / HA and TA@HACC / HA double-layer hydrogel.

[0044] The mechanical strength of the TA@HACC / HA monolayer hydrogel obtained in step (4) was tested using a universal tensile testing machine. Figure 4 As shown; at the same time, its anti-swelling performance was tested, and the results are as follows Figure 3 shown.

[0045] The friction coefficient of the double-layer hydrogel obtained in step (5) against the outer surface, i.e., the HACC / HA surface, was tested using a rheometer. The results are as follows: Figure 5 At the same time, the interface toughness between the adhesive layer and the lubricating layer of the obtained double-layer hydrogel was tested by 180-degree peeling. The experimental results are shown in Figure 6 shown.

[0046] Example 2

[0047] Step (1): Weigh HACC powder and HA powder and mix them evenly in a round-bottom evaporating dish to obtain a uniform composite polysaccharide powder having a repeating unit molar ratio of HACC to HA of 1:0.9, in total two portions.

[0048] Step (2): adding 10 wt% TA and a small amount of water to one portion of the composite polysaccharide powder so that the total molar concentration of HACC and HA repeating units in the mixture is 1.9 mol / L; adding a small amount of GMA (0.006:1), a small amount of KA (0.20:1) and a small amount of water to the other portion of the composite polysaccharide powder so that the total molar concentration of HACC and HA repeating units in the mixture is 1.9 mol / L, and kneading to obtain a HACC / HAC composite dough.

[0049] Step (3): After the composite polysaccharide dough is placed at room temperature (25° C.) for 2.5 hours, it is repeatedly molded-folded-molded three times using a mold consisting of a 0.3 mm PET rectangular frame and a pair of glass plates at room temperature to obtain a transparent and homogeneous precursor sheet.

[0050] Step (4): The precursor sheet was annealed in a constant temperature and humidity chamber at 50° C. for 22 hours to obtain a preformed HACC / HA hydrogel and a preformed TA@HACC / HA hydrogel.

[0051] Step (5): The preformed HACC / HA hydrogel and the preformed TA@HACC / HA hydrogel were molded for 25 minutes, and the HACC / HA surface was irradiated with UV light for 1 hour to fully crosslink the covalently to obtain a multi-hydrogen bond physically crosslinked double-stranded chain structure to obtain a highly entangled HACC / HA and TA@HACC / HA double-layer hydrogel.

[0052] The mechanical strength of the TA@HACC / HA monolayer hydrogel obtained in step (4) was tested using a universal tensile testing machine. Figure 4 As shown; at the same time, its anti-swelling performance was tested, and the results are as follows Figure 3shown.

[0053] The friction coefficient of the double-layer hydrogel obtained in step (5) against the outer surface, i.e., the HACC / HA surface, was tested using a rheometer. The results are as follows: Figure 5 At the same time, the interface toughness between the adhesive layer and the lubricating layer of the obtained double-layer hydrogel was tested by 180-degree peeling. The experimental results are shown in Figure 6 shown.

[0054] Example 3

[0055] Step (1): Weigh HACC powder and HA powder and mix them evenly in a round-bottom evaporating dish to obtain a uniform composite polysaccharide powder having a repeating unit molar ratio of HACC to HA of 1:1.1, in two portions.

[0056] Step (2): Add 12 wt% TA and a small amount of water to one of the composite polysaccharide powders, so that the total molar concentration of HACC and HA repeating units in the mixture is 1.1 mol / L, and knead to obtain TA@HACC / HA composite polysaccharide dough. Add a small amount of GMA (0.008:1), a small amount of KA (0.25:1) and a small amount of water to another composite polysaccharide powder, so that the total molar concentration of HACC and HA repeating units in the mixture is 1.1 mol / L, and knead to obtain HACC / HAC composite dough.

[0057] Step (3): After the composite polysaccharide dough is placed at room temperature (25° C.) for 3 hours, it is repeatedly molded-folded-molded three times at room temperature using a mold consisting of a 0.3 mm PET rectangular frame and a pair of glass plates to obtain a transparent and homogeneous precursor sheet.

[0058] Step (4): The precursor sheet was annealed in a constant temperature and humidity chamber at 50° C. for 20 hours to obtain a preformed HACC / HA hydrogel and a preformed TA@HACC / HA hydrogel.

[0059] Step (5): The preformed HACC / HA hydrogel and the preformed TA@HACC / HA hydrogel were molded for 30 minutes, and the HACC / HA surface was irradiated with UV light for 1 hour to fully crosslink the covalently connected molecules, thereby obtaining a double-stranded chain structure with multiple hydrogen bonds and obtaining a highly entangled HACC / HA and TA@HACC / HA double-layer hydrogel.

[0060] The mechanical strength of the TA@HACC / HA monolayer hydrogel obtained in step (4) was tested using a universal tensile testing machine. Figure 4 As shown; at the same time, its anti-swelling performance was tested, and the results are as follows Figure 3 shown.

[0061] The friction coefficient of the double-layer hydrogel obtained in step (5) against the outer surface, i.e., the HACC / HA surface, was tested using a rheometer. The results are as follows: Figure 5 At the same time, the interface toughness between the adhesive layer and the lubricating layer of the obtained double-layer hydrogel was tested by 180-degree peeling. The experimental results are shown in Figure 6 shown.

[0062] Comparative Example 1

[0063] Step (1): Weigh HA powder into a round-bottom evaporating dish.

[0064] Step (2): HA powder is difficult to aggregate into dough and is in the form of loose sand (water content 50%). Therefore, it is difficult to test the mechanical properties, adhesive properties, and friction coefficient.

[0065] Comparative Example 2

[0066] Step (1): Weigh HACC powder into a round-bottom evaporating dish.

[0067] Step (2): kneading to obtain HACC polysaccharide dough.

[0068] Step (3): After the polysaccharide dough is placed at room temperature (25° C.) for 2 hours, it is repeatedly molded-folded-molded three times using a mold consisting of a 1 mm PET rectangular frame and a pair of glass plates at room temperature to obtain a transparent and homogeneous precursor sheet.

[0069] Step (4): Annealing in a constant temperature and humidity chamber at 50°C for 24 hours to obtain a transparent and homogeneous HA hydrogel.

[0070] The HA gel obtained in this comparative example turned into a soft and weak hydrogel when immersed in deionized water for 1 minute. If the immersion time was further extended, the HA hydrogel disintegrated, so it was difficult to test the friction coefficient. Before equilibration in water, the tensile strength was 0.75MPa, the elongation at break was 315.75%, and the tensile work was 0.017MJ / m 3 , the bonding strength with glass is 11.24kPa.

[0071] Comparative Example 3

[0072] Step (1): Weigh HACC powder into a round-bottom evaporating dish.

[0073] Step (2): adding TA in an amount of 10% of the total mass of the polysaccharide powder to the polysaccharide powder, and kneading to obtain TA@HACC composite polysaccharide dough.

[0074] Step (3): After the polysaccharide dough is placed at room temperature (25° C.) for 2 hours, it is repeatedly molded-folded-molded three times using a mold consisting of a 1 mm PET rectangular frame and a pair of glass plates at room temperature to obtain a transparent and homogeneous precursor sheet.

[0075] Step (4): Annealing in a constant temperature and humidity chamber at 50°C for 24 hours to obtain a transparent and homogeneous TA@HACC hydrogel.

[0076] The volume swelling ratio of the TA@HACC gel obtained in this comparative example after soaking in deionized water for 30 minutes was 12.31 (mm 3 / mm 3 ). Before immersion in water, the tensile strength is 1.38MPa, the elongation at break is 104.45%, and the tensile work is 0.49MJ / m 3 The friction coefficient is 0.28 and the bonding strength to glass is 11.19 kPa.

[0077] Comparative Example 4

[0078] Step (1): Weigh HA powder into a round-bottom evaporating dish.

[0079] Step (2): Add TA in an amount of 10% of the total mass of the polysaccharide powder to the polysaccharide powder, and knead to obtain TA@HA composite polysaccharide dough.

[0080] Step (3): After the polysaccharide dough is placed at room temperature (25° C.) for 2 hours, it is repeatedly molded-folded-molded three times using a mold consisting of a 1 mm PET rectangular frame and a pair of glass plates at room temperature to obtain a transparent and homogeneous precursor sheet.

[0081] Step (4): Annealing was performed in a constant temperature and humidity chamber at 50°C for 24 hours to obtain a transparent and homogeneous TA@HA hydrogel.

[0082] The volume swelling ratio of the TA@HA gel obtained in this comparative example after soaking in deionized water for 20 minutes was 14.05 (mm 3 / mm 3 ), when the immersion time was extended to 30 minutes, the gel began to decompose. The tensile strength before immersion in water was 0.17MPa, the elongation at break was 120.01%, and the tensile work was 0.102MJ / m 3 The friction coefficient is 0.35 and the bonding strength to glass is 13.26 kPa.

[0083] Comparative Example 5

[0084] Step (1): Weigh HACC powder and HA powder and mix them evenly in a round-bottom evaporating dish to obtain a uniform composite polysaccharide powder with a repeating unit molar ratio of HACC to HA of 1:1.

[0085] Step (2): adding water and kneading to obtain a HACC / HA composite polysaccharide dough, wherein the total molar concentration of HACC and HA repeating units is 2.8 mol / L.

[0086] Step (3): After the composite polysaccharide dough is placed at room temperature (25° C.) for 2 hours, it is repeatedly molded-folded-molded three times using a mold consisting of a 0.3 mm PET rectangular frame and a pair of glass plates at room temperature to obtain a transparent and homogeneous precursor sheet.

[0087] Step (4): Then, the mixture was placed in a constant temperature and humidity chamber at 50° C. for annealing for 24 hours to obtain a preformed HACC / HA hydrogel.

[0088] The volume swelling rate of the HACC / HA hydrogel obtained in this comparative example was 1.80 (mm 3 / mm 3 ), before immersion in water, the tensile strength is 0.51MPa, the elongation at break is 275.31%, and the tensile work is 0.899MJ / m 3 The friction coefficient of the HACC / HA layer is 0.05, and the bonding strength with glass is 51.23 kPa.

[0089] Table 1: Volume swelling ratio, tensile strength, stretch ratio, bonding strength, friction coefficient and interface toughness of each hydrogel

[0090]

[0091] The volume swelling ratios of the TA@HACC / HA layer hydrogels in Examples 1 to 3 were 2.80 mm 3 / mm 3 、2.56mm 3 / mm 3 , 2.39mm 3 / mm 3 The average swelling rate is 1.97mm 3 / mm 3 , with strong water swelling resistance. This is because the electrostatic interaction between the HACC and HA molecular chains is transformed into a tightly entangled double-stranded chain structure, and the TA multiple hydrogen bonds synergistically enhance the entanglement between the HACC and HA segments. Comparative Example 1 is difficult to knead into shape, and Comparative Example 2 decomposes rapidly in deionized water. This is because the entanglement formed by only a single segment is weak and it is difficult to maintain a stable structure under external stress. The volume swelling rates of Comparative Examples 3 and 4 are 12.31 mm 3 / mm 3 、14.05mm 3 / mm 3 This is because in Comparative Examples 3 and 4, the main forces are composed of the multiple hydrogen bond enhancement provided by TA and the entanglement of the single strand chain. However, the hydrogen bonds of TA will gradually dissociate in water, and the entanglement of the single strand chain is weak, so Comparative Examples 3 and 4 have a large swelling. The volume swelling rate of Comparative Example 5 is 3.12mm 3 / mm 3, which is higher than that of Examples 1 to 3, indicating that the multiple hydrogen bonds in TA enhance the entanglement of the HACC / HA double strands, thus having a higher stability.

[0092] The tensile strength of comparative example 2 is 0.02MPa, the elongation at break is 122.11%, and the tensile work is 0.01MJ / m 3 This is because the single strand chain relies only on physical entanglement. Although this entanglement can provide a certain mechanical strength, it is very easy to be untied. The tensile strength, elongation at break, and tensile work of Comparative Examples 3 to 4 are 1.38MPa, 0.17MPa, 104.45%, 120.1%, and 0.49MJ / m 3 , 0.012MJ / m 3 When the single strands are strengthened by the hydrogen bonds of TA, the mechanical properties of the gel are improved. Therefore, the tensile strength of Comparative Example 3 is increased compared with Comparative Example 2, and Comparative Example 4 can form a stable gel compared with Comparative Example 1. The tensile strength, elongation at break, and tensile work of Comparative Example 5 are 0.51 MPa, 275.31%, and 0.899 MJ / m respectively. 3 Compared with comparative example 5, examples 1 to 3 exhibit better mechanical properties. Examples 1 to 3 have a tensile strength of 0.95 to 1.90 MPa, an elongation at break of 345.12% to 375.64%, and a tensile work of 0.40 to 0.86 MJ / m 3 The range of changes has an excellent energy dissipation mechanism. This is because the electrostatic interaction between HACC and HA molecular chains is transformed into a tightly wound double-stranded chain structure, and the multiple hydrogen bonds of TA synergistically enhance this structure, thereby enhancing the mechanical properties of the hydrogel material.

[0093] The TA@HACC / HA layers of Examples 1 to 3 and Comparative Examples 2 to 5 were tested for their bonding properties to the glass substrate. The results showed that Examples 1 to 3 all exhibited bonding strengths exceeding 130 kPa, far exceeding Comparative Examples 2 to 5. The bonding properties of Comparative Examples 2 to 4 were 11.24 kPa, 11.19 kPa, and 13.26 kPa, respectively. Compared with Comparative Example 2, the mechanical properties of Comparative Example 3 have greatly increased, but the bonding properties are comparable to those of Comparative Example 2. This is because the hydrogen bonds of TA and the electrostatic interactions between TA and HACC are more used for the stability of the internal structure, such as enhancing entanglement. Compared with Comparative Examples 2 and 3, the bonding properties of Comparative Example 4 have increased because TA and HA carry the same charge, there is no mutual attraction and consumption of positive and negative charges inside, and more functional groups are exposed on the surface. The bonding performance of Comparative Example 5 can reach 51 kPa, because the polyampholyte hydrogels with positive and negative charges have self-adjusting bonding performance, and can be bonded to each other at the interface through the mutual attraction of positive and negative opposite charges through the charge rearrangement of the double electric layer. Examples 1 to 3, based on Comparative Example 5, further introduce multiple hydrogen bonds of TA, which produce a synergistic effect with the electrostatic bonding of polyampholytes, thus showing higher bonding performance, reaching 130.32 kPa, 135.45 kPa, and 132.29 kPa, respectively.

[0094] The friction coefficients of the HA / HACC layer of the embodiment and comparative examples 2 to 5 were tested. The friction coefficients of comparative examples 3 and 4 were 0.28 and 0.35, and the friction coefficient of comparative example 5 was 0.05. The friction coefficients of embodiments 1 to 3 were all 0.05, because the HA / HACC layer formed a dense hydration layer, which gave the gel good lubricity, indicating that it can effectively isolate the adhesion to the outside and tissue.

[0095] The interface toughness results between the adhesive layer and the lubricating layer of the double-layer hydrogels obtained in Examples 1 to 3 showed that the interface toughness of the three groups of experiments all exceeded 50 N / m, among which the interface toughness of the double-layer hydrogel obtained in Example 1 was the highest, reaching 150 N / m.

[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a "adhesive-lubricating double-sided" double-stranded highly entangled polyelectrolyte complex hydrogel, characterized in that: The steps include: (1) chitosan quaternary ammonium salt, hyaluronic acid powder, a cross-linking agent, an initiator, and water are uniformly mixed to obtain a dough-like HACC / HA composite polysaccharide, wherein the molar ratio of the repeating units of chitosan quaternary ammonium salt to hyaluronic acid is 1:0.7-1.3; (2) chitosan quaternary ammonium salt, hyaluronic acid powder, tannic acid and water are uniformly mixed to obtain a dough-like TA@HACC / HA composite polysaccharide, wherein the molar ratio of the repeating units of chitosan quaternary ammonium salt and hyaluronic acid is 1:0.7-1.3; (3) allowing the composite polysaccharide dough obtained in step (1) and step (2) to stand and relax, and then shaping the dough to obtain a sheet-like HACC / HA precursor sheet and a TA@HACC / HA precursor sheet; (4) annealing the obtained precursor sheet to obtain preformed HACC / HA hydrogel and TA@HACC / HA hydrogel; (5) The preformed HACC / HA hydrogel and TA@HACC / HA hydrogel are laminated to initiate polymerization and cross-linking to obtain a highly entangled TA@HACC / HA and HACC / HA double-layer hydrogel with a double-stranded chain structure physically cross-linked by multiple hydrogen bonds.

2. The preparation method according to claim 1, characterized in that: The mixing method in step (1) and step (2) is selected from one of stirring, kneading, beating, and repeated molding-folding-molding or a combination thereof.

3. The preparation method according to claim 1, characterized in that: The tannic acid content in the TA@HACC / HA composite polysaccharide obtained in step (2) is 8wt%-14wt%.

4. The preparation method according to claim 1, characterized in that: The ratio of the molar concentration of the crosslinking agent to the total molar concentration of the repeating units of the polysaccharide quaternary ammonium salt and hyaluronic acid is (0.004-0.008):1; the ratio of the molar concentration of the initiator to the molar concentration of methacrylate glycerol is (0.15-0.25):

1.

5. The preparation method according to claim 1, characterized in that: The crosslinking agent is glyceryl methacrylate, and the initiator is α-ketoglutaric acid.

6. The preparation method according to claim 1, characterized in that: In the HACC / HA composite polysaccharide obtained in step (1), the total molar concentration of repeating units of chitosan quaternary ammonium salt and hyaluronic acid is 1.1-2.8 mol / L; in the TA@HACC / HA composite polysaccharide obtained in step (2), the total molar concentration of repeating units of chitosan quaternary ammonium salt and hyaluronic acid is 1.1-2.8 mol / L.

7. The preparation method according to claim 1, characterized in that: The temperature of the standing relaxation treatment in step (3) is 10 to 40° C., and the time is 0.1 to 3 hours; the temperature of the annealing treatment in step (4) is 50 to 60° C., and the time of the annealing treatment is 12 to 24 hours.

8. The preparation method according to claim 1, characterized in that: The thickness of the HACC / HA precursor sheet and the TA@HACC / HA precursor sheet obtained in step (3) is 0.1 to 3 mm.

9. A "adhesive-lubricating double-sided" double-stranded highly entangled polyelectrolyte complex hydrogel, characterized in that: The method is prepared by any one of claims 1 to 8.

10. The use of the "adhesive-lubricating dual-sided" double-stranded highly entangled polyelectrolyte complex hydrogel according to claim 9, characterized in that: Used to prepare artificial biological internal tissue wound replacement materials.